MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Covestro Makrolon® DP1-1821 Polycarbonate
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Molded

Material Notes: MVR (300 °C/1.2 kg) 6.0 cm³/10 min; lenses, optical; high viscosity; UV stabilized; easy release; high purity; injection molding - melt temperature 280 - 320 °C; available in clear tints only

As of 1 September 2015, Bayer MaterialScience was separated from Bayer AG and officially adopted its new name – Covestro.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 0.660 g/cc0.0238 lb/in³pellets; ISO 60
Density 1.20 g/cc0.0434 lb/in³ISO 1183
Moisture Absorption at Equilibrium 0.12 %0.12 %ISO 62
Water Absorption at Saturation 0.30 %0.30 %ISO 62
Linear Mold Shrinkage 0.0060 - 0.0080 cm/cm0.0060 - 0.0080 in/inparallel/normal; b.o. ISO 2577
Linear Mold Shrinkage, Flow 0.0070 cm/cm0.0070 in/in60x60x2 mm; 500 bar; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0075 cm/cm0.0075 in/in60x60x2 mm; 500 bar; ISO 294-4
Melt Flow 6.5 g/10 min
@Load 1.20 kg,
Temperature 300 °C
6.5 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 114 MPa16500 psiISO 2039-1
Tensile Strength at Break 70.0 MPa10200 psi50 mm/min; ISO 527-1/-2
Tensile Strength, Yield 66.0 MPa9570 psi50 mm/min; ISO 527-1/-2
Elongation at Break >= 50 %>= 50 %Nominal, 50 mm/min; ISO 527-1/-2
 130 %130 %50 mm/min; ISO 527-1/-2
Elongation at Yield 6.2 %6.2 %50 mm/min; ISO 527-1/-2
Tensile Modulus 2.40 GPa348 ksi1 mm/min; ISO 527-1/-2
Flexural Strength 98.0 MPa14200 psi2 mm/min; ISO 178
Flexural Yield Strength 74.0 MPa
@Strain 3.4 %
10700 psi
@Strain 3.4 %
2 mm/min; ISO 178
Flexural Modulus 2.40 GPa348 ksi2 mm/min; ISO 178
Flexural Strain at Yield 7.0 %7.0 %2 mm/min; ISO 178
Izod Impact, Notched (ISO)  15.0 kJ/m²
@Thickness 3.00 mm,
Temperature -30.0 °C
7.14 ft-lb/in²
@Thickness 0.118 in,
Temperature -22.0 °F
complete break; ISO 7391/b.o. ISO 180-A
 70.0 kJ/m²
@Thickness 3.00 mm,
Temperature 23.0 °C
33.3 ft-lb/in²
@Thickness 0.118 in,
Temperature 73.4 °F
partial break; ISO 7391/b.o. ISO 180-A
Charpy Impact Unnotched NBNBISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
 NB
@Temperature -60.0 °C
NB
@Temperature -76.0 °F
ISO 179/1eU
Charpy Impact, Notched  1.40 J/cm²
@Thickness 3.00 mm,
Temperature -30.0 °C
6.66 ft-lb/in²
@Thickness 0.118 in,
Temperature -22.0 °F
complete break; ISO 7391/b.o. ISO 179-1eA
 8.00 J/cm²
@Thickness 3.00 mm,
Temperature 23.0 °C
38.1 ft-lb/in²
@Thickness 0.118 in,
Temperature 73.4 °F
partial break; ISO 7391/b.o. ISO 179-1eA
Impact 55005500Puncture - maximum force (N); ISO 6603-2
 6500
@Temperature -30.0 °C
6500
@Temperature -22.0 °F
Puncture - maximum force (N); ISO 6603-2
Puncture Energy 60.0 J44.3 ft-lbISO 6603-2
 70.0 J
@Temperature -30.0 °C
51.6 ft-lb
@Temperature -22.0 °F
ISO 6603-2
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+13 ohm-cm>= 1.00e+13 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 60093
Dielectric Constant  3.0
@Frequency 1e+6 Hz
3.0
@Frequency 1e+6 Hz
IEC 60250
 3.1
@Frequency 100 Hz
3.1
@Frequency 100 Hz
IEC 60250
Dielectric Strength 34.0 kV/mm864 kV/inIEC 60243-1
Dissipation Factor  0.00050
@Frequency 100 Hz
0.00050
@Frequency 100 Hz
IEC 60250
 0.0095
@Frequency 1e+6 Hz
0.0095
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 250 V250 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 65.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
36.1 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 65.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
36.1 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1/-2
Thermal Conductivity 0.200 W/m-K1.39 BTU-in/hr-ft²-°Fcross-flow; ISO 8302
Hot Ball Pressure Test 137 °C279 °FIEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 138 °C280 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 125 °C257 °FISO 75-1/-2
Vicat Softening Point 144 °C291 °F50°C/h 50N; ISO 306
 147 °C297 °F50 N; 120 °C/h; ISO 306
Glass Transition Temp, Tg 145 °C293 °FISO 11357-1/-2
Flash Point 480 °C896 °Fignition; ASTM D1929
 550 °C1020 °Fself ignition; ASTM D1929
Oxygen Index 27 %27 %Method A; ISO 4589-1/-2
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.5861.586ISO 489
Transmission, Visible  88 %
@Thickness 3.00 mm
88 %
@Thickness 0.118 in
ISO 13468-2
 89 %
@Thickness 1.00 mm
89 %
@Thickness 0.0394 in
ISO 13468-2
 89 %
@Thickness 2.00 mm
89 %
@Thickness 0.0787 in
ISO 13468-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 300 °C572 °FInjection Molding; ISO 294
Mold Temperature 80.0 °C176 °FInjection Molding; ISO 294
Injection Velocity 200 mm/sec7.87 in/secISO 294
 
Descriptive Properties
AvailabilityAsia Pacific
 India
 North America
FeatureLight stabilized or stable to light
 Release agent
 U.V. stabilized or stable to weather
FormPellets
ProcessInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Covestro Makrolon® LQ2647 Optical Grade Polycarbonate
Covestro Apec® 1695 Polycarbonate
Covestro Makrolon® 1248 Polycarbonate, Impact Grade
Covestro Makrolon® 1804 Polycarbonate
Covestro Makrolon® 1952 Polycarbonate

PB09949 / 92789

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.