MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LG Chemical LUMID EG2308BW PA66+GF30%, Injection Molding
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: Chemical Resistance (Ethylene Glycol), Hydrolysis Resistance

Application: Radiator End Tank, Intercooler (Outlet )

Information provided by LG Chemical

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.36 g/cc0.0491 lb/in³ISO 1183
Moisture Absorption 2.0 %2.0 %50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0040 cm/cm
@Thickness 2.00 mm
0.0040 in/in
@Thickness 0.0787 in
Internal pressure 60MPa; ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 190 MPa27600 psi5mm/min; ISO 527
Elongation at Break 3.3 %3.3 %5mm/min; ISO 527
Flexural Strength 255 MPa37000 psi2mm/min; ISO 178
Flexural Modulus 8.50 GPa1230 ksi2mm/min; ISO 178
Izod Impact, Notched (ISO)  9.00 kJ/m²
@Temperature -30.0 °C
4.28 ft-lb/in²
@Temperature -22.0 °F
80*10*4mm; ISO 180/1A
 11.0 kJ/m²
@Temperature 23.0 °C
5.23 ft-lb/in²
@Temperature 73.4 °F
80*10*4mm; ISO 180/1A
Izod Impact, Unnotched (ISO)  55.0 kJ/m²
@Temperature -30.0 °C
26.2 ft-lb/in²
@Temperature -22.0 °F
80*10*4mm; ISO 180/1A
 75.0 kJ/m²
@Temperature 23.0 °C
35.7 ft-lb/in²
@Temperature 73.4 °F
80*10*4mm; ISO 180/1A
Charpy Impact Unnotched  5.50 J/cm²
@Temperature -30.0 °C
26.2 ft-lb/in²
@Temperature -22.0 °F
80*10*4mm; ISO179/1eA
 7.50 J/cm²
@Temperature 23.0 °C
35.7 ft-lb/in²
@Temperature 73.4 °F
80*10*4mm; ISO179/1eA
Charpy Impact, Notched  0.900 J/cm²
@Temperature -30.0 °C
4.28 ft-lb/in²
@Temperature -22.0 °F
80*10*4mm; ISO179/1eA
 1.10 J/cm²
@Temperature 23.0 °C
5.23 ft-lb/in²
@Temperature 73.4 °F
80*10*4mm; ISO179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+13 ohm-cm1.00e+13 ohm-cmIEC 60093
Dielectric Strength 35.0 kV/mm
@Thickness 1.00 mm
889 kV/in
@Thickness 0.0394 in
EC 60243-1
 
Thermal PropertiesMetricEnglishComments
Melting Point 260 °C500 °FISO 11357
Deflection Temperature at 0.46 MPa (66 psi) 255 °C491 °FUnannealed, Edge; SO 75
Deflection Temperature at 1.8 MPa (264 psi) 245 °C473 °FUnannealed, Edge; SO 75
Flammability, UL94 HB
@Thickness 0.750 mm
HB
@Thickness 0.0295 in
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 260 - 270 °C500 - 518 °F
Middle Barrel Temperature 270 - 285 °C518 - 545 °F
Front Barrel Temperature 270 - 290 °C518 - 554 °F
Nozzle Temperature 270 - 295 °C518 - 563 °F
Melt Temperature 270 - 295 °C518 - 563 °F
Mold Temperature 80.0 - 100 °C176 - 212 °F
Drying Temperature 80.0 - 90.0 °C
@Time 14400 - 18000 sec
176 - 194 °F
@Time 4.00 - 5.00 hour
Moisture Content <= 0.12 %<= 0.12 %
Back Pressure 0.981 - 2.94 MPa142 - 426 psiHydraulic
 9.81 - 29.4 MPa1420 - 4260 psiElectronic
Screw Speed 60 - 200 rpm60 - 200 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LG Chemical LUMID GP2301BFH PA66+GF30%, Injection Molding
LG Chemical LUMID EG2309B(W) PA66+GF30%, Chemical Resistance(CaCl2, Ethylene Glycol)
LG Chemical LUMID GP2130A(W) PA6+GF13%, General Purpose
LG Chemical LUMID GP2251BF PA66+GF25%, Flame Retardant
LG Chemical LUMID GP2300B PA66+GF30%, Injection Molding

PLHCHEM9749 / 239265

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.