AISI Type 410S Stainless Steel, tempered at 733°C
Categories:
Metal
;
Ferrous Metal
;
Heat Resisting
;
Stainless Steel
;
T 400 Series Stainless Steel
Material Notes:
16 mm diameter bar, heated to 980°C for 30 min., oil quenched, test temperature plus 28°C temper for 2 hours
Key Words:
ASME SA240, ASTM A176, ASTM A240, ASTM A473, DIN 1.4001, JIS SUS 410 S, B.S. 403 S 17, martensitic
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
7.80
g/cc
0.282
lb/in³
Mechanical Properties
Metric
English
Comments
Tensile Strength, Ultimate
195
MPa
@Temperature 705 °C
28300
psi
@Temperature 1300 °F
Tensile Strength, Yield
165
MPa
@Strain 0.2 %
23900
psi
@Strain 0.2 %
165
MPa
@Strain 0.2 %,
Temperature 705 °C
23900
psi
@Strain 0.2 %,
Temperature 1300 °F
Elongation at Break
24 %
@Temperature 705 °C
24 %
@Temperature 1300 °F
in 50 mm
Modulus of Elasticity
200
GPa
29000
ksi
Annealed AISI 410
Electrical Properties
Metric
English
Comments
Electrical Resistivity
0.0000570
ohm-cm
@Temperature 20.0 °C
0.0000570
ohm-cm
@Temperature 68.0 °F
0.000108
ohm-cm
@Temperature 650 °C
0.000108
ohm-cm
@Temperature 1200 °F
Thermal Properties
Metric
English
Comments
CTE, linear
9.90
µm/m-°C
@Temperature 0.000 - 100 °C
5.50
µin/in-°F
@Temperature 32.0 - 212 °F
11.0
µm/m-°C
@Temperature 0.000 - 315 °C
6.11
µin/in-°F
@Temperature 32.0 - 599 °F
11.5
µm/m-°C
@Temperature 0.000 - 540 °C
6.39
µin/in-°F
@Temperature 32.0 - 1000 °F
11.7
µm/m-°C
@Temperature 0.000 - 650 °C
6.50
µin/in-°F
@Temperature 32.0 - 1200 °F
Specific Heat Capacity
0.460
J/g-°C
@Temperature 0.000 - 100 °C
0.110
BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity
24.9
W/m-K
@Temperature 100 °C
173
BTU-in/hr-ft²-°F
@Temperature 212 °F
28.7
W/m-K
@Temperature 500 °C
199
BTU-in/hr-ft²-°F
@Temperature 932 °F
Melting Point
1480
-
1530
°C
2700
-
2790
°F
Solidus
1480
°C
2700
°F
Liquidus
1530
°C
2790
°F
Maximum Service Temperature, Air
705
°C
1300
°F
Continuous Service
815
°C
1500
°F
Intermittent
Component Elements Properties
Metric
English
Comments
Carbon, C
<= 0.080 %
<= 0.080 %
Chromium, Cr
12.5 %
12.5 %
Iron, Fe
85 %
85 %
Manganese, Mn
<= 1.0 %
<= 1.0 %
Phosphorus, P
<= 0.040 %
<= 0.040 %
Silicon, Si
<= 1.0 %
<= 1.0 %
Sulfur, S
<= 0.030 %
<= 0.030 %
References
for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
AISI Type 410S Stainless Steel, tempered at 568°C
AISI Type 410S Stainless Steel, tempered at 623°C
AISI Type 410S Stainless Steel, tempered at 678°C
410 Stainless Steel, tempered at 650°C
AISI Type 410S Stainless Steel, tempered at 508°C
MQ410CI / 12989
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.