MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Celanese Zytel® HTN 51G50HSL BK083 Polyphthalamide (PPA) (Extended Tabular Stress-Strain Data)
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), 50% Glass Fiber Reinforced

Material Notes: Zytel® HTN51G50HSL BK083 is a 50% glass reinforced, heat stabilized, lubricated high performance polyamide resin. It is also a PPA resin.

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.45 g/cc0.0524 lb/in³DAM; ISO 1183
 1.64 g/cc0.0592 lb/in³DAM; ISO 1183
Filler Content 50 %50 %DAM
Melt Density 1.10 g/cc
@Temperature 325 °C
0.0397 lb/in³
@Temperature 617 °F
Water Absorption 0.30 %
@Temperature 23.0 °C
0.30 %
@Temperature 73.4 °F
Immersion 24h; DAM; ISO 62, Similar to
 0.40 %
@Time 86400 sec
0.40 %
@Time 24.0 hour
Immersion; DS; DAM; Sim. to ISO 62
Moisture Absorption 2.00 %
@Thickness 2.00 mm
2.00 %
@Thickness 0.0787 in
DAM; Sim. to ISO 62
Viscosity Number 120 cm³/g1.20 dl/gDAM; ISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.0030 cm/cm0.0030 in/inDAM; ISO 294-4, 2577
 0.0020 cm/cm
@Thickness 2.00 mm
0.0020 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0090 cm/cm0.0090 in/inDAM; ISO 294-4, 2577
 0.0050 cm/cm
@Thickness 2.00 mm
0.0050 in/in
@Thickness 0.0787 in
DAM; ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 180 MPa26100 psi50% RH; ISO 527-1/-2
 210 MPa30500 psiDAM; ISO 527-1/-2
 245 MPa
@Temperature 23.0 °C
35500 psi
@Temperature 73.4 °F
50%RH; ISO 527
 262 MPa
@Temperature 23.0 °C
38000 psi
@Temperature 73.4 °F
DAM; ISO 527
Tensile Stress at Strain  8.38 MPa
@Strain 0.1 %,
Temperature 150 °C
1220 psi
@Strain 0.1 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 16.74 MPa
@Strain 0.2 %,
Temperature 150 °C
2428 psi
@Strain 0.2 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 16.9 MPa
@Strain 0.1 %,
Temperature 100 °C
2450 psi
@Strain 0.1 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 18.64 MPa
@Strain 0.1 %,
Temperature -40.0 °C
2704 psi
@Strain 0.1 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 18.85 MPa
@Strain 0.1 %,
Temperature 23.0 °C
2734 psi
@Strain 0.1 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 23.75 MPa
@Strain 0.3 %,
Temperature 150 °C
3445 psi
@Strain 0.3 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 28.94 MPa
@Strain 0.4 %,
Temperature 150 °C
4197 psi
@Strain 0.4 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 33.24 MPa
@Strain 0.2 %,
Temperature 100 °C
4821 psi
@Strain 0.2 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 36.41 MPa
@Strain 0.2 %,
Temperature 23.0 °C
5281 psi
@Strain 0.2 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 36.55 MPa
@Strain 0.5 %,
Temperature 150 °C
5301 psi
@Strain 0.5 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 36.98 MPa
@Strain 0.2 %,
Temperature -40.0 °C
5364 psi
@Strain 0.2 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 41.74 MPa
@Strain 0.6 %,
Temperature 150 °C
6054 psi
@Strain 0.6 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 46.06 MPa
@Strain 0.7 %,
Temperature 150 °C
6680 psi
@Strain 0.7 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 48.4 MPa
@Strain 0.3 %,
Temperature 100 °C
7020 psi
@Strain 0.3 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 49.39 MPa
@Strain 0.8 %,
Temperature 150 °C
7163 psi
@Strain 0.8 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 52.38 MPa
@Strain 0.9 %,
Temperature 150 °C
7597 psi
@Strain 0.9 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 53.72 MPa
@Strain 0.3 %,
Temperature 23.0 °C
7791 psi
@Strain 0.3 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 55.0 MPa
@Strain 1 %,
Temperature 150 °C
7980 psi
@Strain 1 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 55.26 MPa
@Strain 0.3 %,
Temperature -40.0 °C
8015 psi
@Strain 0.3 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 57.24 MPa
@Strain 1.1 %,
Temperature 150 °C
8302 psi
@Strain 1.1 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 59.17 MPa
@Strain 1.2 %,
Temperature 150 °C
8582 psi
@Strain 1.2 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 60.99 MPa
@Strain 0.4 %,
Temperature 100 °C
8846 psi
@Strain 0.4 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 61.0 MPa
@Strain 1.3 %,
Temperature 150 °C
8850 psi
@Strain 1.3 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 62.49 MPa
@Strain 1.4 %,
Temperature 150 °C
9063 psi
@Strain 1.4 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 63.82 MPa
@Strain 1.5 %,
Temperature 150 °C
9256 psi
@Strain 1.5 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 65.13 MPa
@Strain 1.6 %,
Temperature 150 °C
9446 psi
@Strain 1.6 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 66.11 MPa
@Strain 1.7 %,
Temperature 150 °C
9588 psi
@Strain 1.7 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 67.32 MPa
@Strain 1.8 %,
Temperature 150 °C
9764 psi
@Strain 1.8 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 67.86 MPa
@Strain 0.4 %,
Temperature 23.0 °C
9842 psi
@Strain 0.4 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 68.09 MPa
@Strain 1.9 %,
Temperature 150 °C
9876 psi
@Strain 1.9 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 68.92 MPa
@Strain 2 %,
Temperature 150 °C
9996 psi
@Strain 2 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 69.59 MPa
@Strain 2.1 %,
Temperature 150 °C
10090 psi
@Strain 2.1 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 70.26 MPa
@Strain 0.4 %,
Temperature -40.0 °C
10190 psi
@Strain 0.4 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 70.34 MPa
@Strain 2.2 %,
Temperature 150 °C
10200 psi
@Strain 2.2 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 70.9 MPa
@Strain 2.3 %,
Temperature 150 °C
10300 psi
@Strain 2.3 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 71.53 MPa
@Strain 2.4 %,
Temperature 150 °C
10370 psi
@Strain 2.4 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 72.01 MPa
@Strain 2.5 %,
Temperature 150 °C
10440 psi
@Strain 2.5 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 72.83 MPa
@Strain 2.6 %,
Temperature 150 °C
10560 psi
@Strain 2.6 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 73.58 MPa
@Strain 2.7 %,
Temperature 150 °C
10670 psi
@Strain 2.7 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 73.73 MPa
@Strain 2.8 %,
Temperature 150 °C
10690 psi
@Strain 2.8 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 73.85 MPa
@Strain 2.9 %,
Temperature 150 °C
10710 psi
@Strain 2.9 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 74.25 MPa
@Strain 3 %,
Temperature 150 °C
10770 psi
@Strain 3 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 74.39 MPa
@Strain 3.1 %,
Temperature 150 °C
10790 psi
@Strain 3.1 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 74.78 MPa
@Strain 3.2 %,
Temperature 150 °C
10850 psi
@Strain 3.2 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 74.98 MPa
@Strain 3.3 %,
Temperature 150 °C
10870 psi
@Strain 3.3 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 75.25 MPa
@Strain 3.4 %,
Temperature 150 °C
10910 psi
@Strain 3.4 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 75.52 MPa
@Strain 3.5 %,
Temperature 150 °C
10950 psi
@Strain 3.5 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 75.65 MPa
@Strain 3.6 %,
Temperature 150 °C
10970 psi
@Strain 3.6 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 75.95 MPa
@Strain 3.7 %,
Temperature 150 °C
11020 psi
@Strain 3.7 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 76.0 MPa
@Strain 3.8 %,
Temperature 150 °C
11000 psi
@Strain 3.8 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 76.23 MPa
@Strain 4.3 %,
Temperature 150 °C
11060 psi
@Strain 4.3 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 76.28 MPa
@Strain 3.9 %,
Temperature 150 °C
11060 psi
@Strain 3.9 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 76.32 MPa
@Strain 4 %,
Temperature 150 °C
11070 psi
@Strain 4 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 76.43 MPa
@Strain 4.1 %,
Temperature 150 °C
11090 psi
@Strain 4.1 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 76.48 MPa
@Strain 4.2 %,
Temperature 150 °C
11090 psi
@Strain 4.2 %,
Temperature 302 °F
DAM; ISO 11403-1/-2
 77.92 MPa
@Strain 0.5 %,
Temperature 100 °C
11300 psi
@Strain 0.5 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 87.6 MPa
@Strain 0.5 %,
Temperature 23.0 °C
12700 psi
@Strain 0.5 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 90.34 MPa
@Strain 0.6 %,
Temperature 100 °C
13100 psi
@Strain 0.6 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 91.29 MPa
@Strain 0.5 %,
Temperature -40.0 °C
13240 psi
@Strain 0.5 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 101.72 MPa
@Strain 0.7 %,
Temperature 100 °C
14753 psi
@Strain 0.7 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 103.36 MPa
@Strain 0.6 %,
Temperature 23.0 °C
14991 psi
@Strain 0.6 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 108.57 MPa
@Strain 0.6 %,
Temperature -40.0 °C
15747 psi
@Strain 0.6 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 111.91 MPa
@Strain 0.8 %,
Temperature 100 °C
16231 psi
@Strain 0.8 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 118.75 MPa
@Strain 0.7 %,
Temperature 23.0 °C
17223 psi
@Strain 0.7 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 120.38 MPa
@Strain 0.9 %,
Temperature 100 °C
17460 psi
@Strain 0.9 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 124.19 MPa
@Strain 0.7 %,
Temperature -40.0 °C
18012 psi
@Strain 0.7 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 127.59 MPa
@Strain 1 %,
Temperature 100 °C
18505 psi
@Strain 1 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 132.6 MPa
@Strain 0.8 %,
Temperature 23.0 °C
19230 psi
@Strain 0.8 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 134.78 MPa
@Strain 1.1 %,
Temperature 100 °C
19548 psi
@Strain 1.1 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 140.54 MPa
@Strain 1.2 %,
Temperature 100 °C
20384 psi
@Strain 1.2 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 140.97 MPa
@Strain 0.8 %,
Temperature -40.0 °C
20446 psi
@Strain 0.8 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 145.44 MPa
@Strain 1.3 %,
Temperature 100 °C
21094 psi
@Strain 1.3 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 146.2 MPa
@Strain 0.9 %,
Temperature 23.0 °C
21200 psi
@Strain 0.9 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 149.84 MPa
@Strain 1.4 %,
Temperature 100 °C
21732 psi
@Strain 1.4 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 153.62 MPa
@Strain 1.5 %,
Temperature 100 °C
22281 psi
@Strain 1.5 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 156.75 MPa
@Strain 0.9 %,
Temperature -40.0 °C
22735 psi
@Strain 0.9 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 156.86 MPa
@Strain 1.6 %,
Temperature 100 °C
22751 psi
@Strain 1.6 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 158.64 MPa
@Strain 1 %,
Temperature 23.0 °C
23009 psi
@Strain 1 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 159.52 MPa
@Strain 1.7 %,
Temperature 100 °C
23136 psi
@Strain 1.7 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 161.9 MPa
@Strain 1.8 %,
Temperature 100 °C
23480 psi
@Strain 1.8 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 163.86 MPa
@Strain 1.9 %,
Temperature 100 °C
23766 psi
@Strain 1.9 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 165.36 MPa
@Strain 2 %,
Temperature 100 °C
23983 psi
@Strain 2 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 166.47 MPa
@Strain 2.1 %,
Temperature 100 °C
24144 psi
@Strain 2.1 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 167 MPa
@Strain 2.2 %,
Temperature 100 °C
24200 psi
@Strain 2.2 %,
Temperature 212 °F
DAM; ISO 11403-1/-2
 170.36 MPa
@Strain 1.1 %,
Temperature 23.0 °C
24709 psi
@Strain 1.1 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 171.78 MPa
@Strain 1 %,
Temperature -40.0 °C
24915 psi
@Strain 1 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 181.45 MPa
@Strain 1.2 %,
Temperature 23.0 °C
26317 psi
@Strain 1.2 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 186.04 MPa
@Strain 1.1 %,
Temperature -40.0 °C
26983 psi
@Strain 1.1 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 191.86 MPa
@Strain 1.3 %,
Temperature 23.0 °C
27827 psi
@Strain 1.3 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 199.84 MPa
@Strain 1.2 %,
Temperature -40.0 °C
28984 psi
@Strain 1.2 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 201.7 MPa
@Strain 1.4 %,
Temperature 23.0 °C
29250 psi
@Strain 1.4 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 210.84 MPa
@Strain 1.5 %,
Temperature 23.0 °C
30580 psi
@Strain 1.5 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 213.16 MPa
@Strain 1.3 %,
Temperature -40.0 °C
30916 psi
@Strain 1.3 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 219.08 MPa
@Strain 1.6 %,
Temperature 23.0 °C
31775 psi
@Strain 1.6 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 225.72 MPa
@Strain 1.4 %,
Temperature -40.0 °C
32738 psi
@Strain 1.4 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 226.7 MPa
@Strain 1.7 %,
Temperature 23.0 °C
32880 psi
@Strain 1.7 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 233.9 MPa
@Strain 1.8 %,
Temperature 23.0 °C
33920 psi
@Strain 1.8 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 237.73 MPa
@Strain 1.5 %,
Temperature -40.0 °C
34480 psi
@Strain 1.5 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 240.33 MPa
@Strain 1.9 %,
Temperature 23.0 °C
34857 psi
@Strain 1.9 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 245.97 MPa
@Strain 2 %,
Temperature 23.0 °C
35675 psi
@Strain 2 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 249.34 MPa
@Strain 1.6 %,
Temperature -40.0 °C
36164 psi
@Strain 1.6 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 251.1 MPa
@Strain 2.1 %,
Temperature 23.0 °C
36420 psi
@Strain 2.1 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 255.01 MPa
@Strain 2.2 %,
Temperature 23.0 °C
36986 psi
@Strain 2.2 %,
Temperature 73.4 °F
DAM; ISO 11403-1/-2
 260.39 MPa
@Strain 1.7 %,
Temperature -40.0 °C
37766 psi
@Strain 1.7 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 270.88 MPa
@Strain 1.8 %,
Temperature -40.0 °C
39288 psi
@Strain 1.8 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 280.96 MPa
@Strain 1.9 %,
Temperature -40.0 °C
40750 psi
@Strain 1.9 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 290.6 MPa
@Strain 2 %,
Temperature -40.0 °C
42150 psi
@Strain 2 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 299.59 MPa
@Strain 2.1 %,
Temperature -40.0 °C
43452 psi
@Strain 2.1 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 307.99 MPa
@Strain 2.2 %,
Temperature -40.0 °C
44670 psi
@Strain 2.2 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 315.88 MPa
@Strain 2.3 %,
Temperature -40.0 °C
45815 psi
@Strain 2.3 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
 321.27 MPa
@Strain 2.4 %,
Temperature -40.0 °C
46596 psi
@Strain 2.4 %,
Temperature -40.0 °F
DAM; ISO 11403-1/-2
Elongation at Break 2.6 %2.6 %50% RH; ISO 527-1/-2
 2.6 %2.6 %DAM; ISO 527-1/-2
 2.1 %
@Temperature 23.0 °C
2.1 %
@Temperature 73.4 °F
DAM; ISO 527
 2.1 %
@Temperature 23.0 °C
2.1 %
@Temperature 73.4 °F
50%RH; ISO 527
Tensile Modulus 12.0 GPa1740 ksiDS; 50% RH; ISO 527-1/-2
 12.0 GPa1740 ksiDS; DAM; ISO 527-1/-2
 17.8 GPa
@Temperature 23.0 °C
2580 ksi
@Temperature 73.4 °F
DAM; ISO 527
 17.8 GPa
@Temperature 23.0 °C
2580 ksi
@Temperature 73.4 °F
50%RH; ISO 527
Flexural Strength 290 MPa42100 psiDAM; ISO 178
Flexural Modulus 10.4 GPa1510 ksiDAM; ISO 178
 16.4 GPa
@Temperature 23.0 °C
2380 ksi
@Temperature 73.4 °F
DAM; ISO 178
Poissons Ratio 0.330.3350% RH
 0.330.33DAM
Charpy Impact Unnotched  6.00 J/cm²
@Temperature 23.0 °C
28.6 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eU
 8.00 J/cm²
@Temperature 23.0 °C
38.1 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eU
Charpy Impact, Notched  1.00 J/cm²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
 1.50 J/cm²
@Temperature 23.0 °C
7.14 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
 1.50 J/cm²
@Temperature -40.0 °C
7.14 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmDAM; IEC 62631-3-1
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohm50% RH; IEC 62631-3-2
Dielectric Constant  4.2
@Frequency 1e+6 Hz
4.2
@Frequency 1e+6 Hz
DAM; IEC 62631-2-1
 4.3
@Frequency 100 Hz
4.3
@Frequency 100 Hz
DAM; IEC 62631-2-1
Dielectric Strength 30.0 kV/mm762 kV/in50% RH; IEC 60243-1
 31.0 kV/mm787 kV/inDAM; IEC 60243-1
Comparative Tracking Index 600 V600 VDAM; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 20.0 µm/m-°C11.1 µin/in-°FDAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 65.0 µm/m-°C36.1 µin/in-°FDAM; ISO 11359-1/-2
 45.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
25.0 µin/in-°F
@Temperature -40.0 - 73.4 °F
DAM; ISO 11359-1/-2
 48.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
26.7 µin/in-°F
@Temperature 73.4 - 131 °F
DAM; ISO 11359-1/-2
 53.0 µm/m-°C
@Temperature 55.0 - 110 °C
29.4 µin/in-°F
@Temperature 131 - 230 °F
DAM; ISO 11359-1/-2
 70.0 µm/m-°C
@Temperature 160 - 200 °C
38.9 µin/in-°F
@Temperature 320 - 392 °F
DAM; ISO 11359-1/-2
Thermal Conductivity 0.240 W/m-K
@Temperature 325 °C
1.67 BTU-in/hr-ft²-°F
@Temperature 617 °F
Melt
Melting Point 300 °C572 °F10°C/min, First Heat; DAM; ISO 11357-1/-3
 310 °C590 °Ffirst heat; DAM; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 265 °C509 °FDAM; ISO 75-1/-2
 285 °C545 °FDAM; ISO 75-1/-2
Glass Transition Temp, Tg 45.0 °C113 °F10°C/min; 50% RH; ISO 11357-1/-2
 90.0 °C194 °F10°C/min; DAM; ISO 11357-1/-2
Flame Spread 44.0 mm/min
@Thickness 1.00 mm
1.73 in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
Oxygen Index 23 %23 %DAM; ISO 4589-1/-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 325 °C617 °FOptimum, Injection
 320 - 330 °C608 - 626 °FRange, Injection
 320 - 330 °C608 - 626 °FDAM
 325 °C617 °FDAM; Optimum
Mold Temperature 90.0 - 110 °C194 - 230 °FInjection
 140 - 160 °C284 - 320 °FDAM
 150 °C302 °FDAM; optimum
Drying Temperature 100 °C212 °FInjection
 100 °C212 °FDAM
Dry Time 6.00 - 8.00 hour6.00 - 8.00 hourInjection, Dehumidified Dryer
 6.00 - 8.00 hour6.00 - 8.00 hourDAM
Moisture Content <= 0.10 %<= 0.10 %Injection
 <= 0.10 %<= 0.10 %DAM
 
Descriptive Properties
AppearanceBlack ColorDAM
FillerGlass Fiber reinforcementDAM
FormsPelletsDAM
GenericPolyphthalamide (PPA)DAM
Material StatusPreliminary DataDAM
Part Marking Code>PA6T/XT-GF50<ISO 11469; DAM
 >PPA-GF50<SAE J1344; DAM
Polymer FamilyHigh performance polyamideDAM
Polymer TypePartially Aromatic PA, PPADAM
Processing MethodInjection MoldingDAM
Product CategoryGlass Reinforced ResinsDAM
 Superstructural ResinsDAM
Region Available - GlobalYesDAM
Resin IdentificationPA6T/XT-GF50ISO 1043; DAM

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Zytel® HTN 55G55LWSF BK752A Polyphthalamide (PPA)
Celanese Zytel® HTN 51G50HSL BK083 Polyphthalamide (PPA)
Akro-Plastic Akromid® T1 GF 50 9 (3257) PPA Dry, 50% Glass Filled
DuPont Mobility and Materials Zytel® HTN FR52G20NH BK337 Polyphthalamide (PPA)
Aluminum 6061-T6; 6061-T651

PDSZ1423a / 234776

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.