MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Atom Adhesives AA-DUCT N02 Epoxy Adhesive
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: AA-DUCT N02 is a single component, heat curing, conductive epoxy polymer that was designed for ease in handling. This high performance conductive polymer cures quickly at elevated temperatures making it ideally suited for rapid Processing and assembly. AA-DUCT N02 passes NASA’s outgassing testing (ASTM E-595) and is listed in NASA’s Outgassing Data for Selecting Spacecraft Materials list. AA-DUCT N02 offers excellent mechanical, electrical, and physical properties at continuous operating Temperatures up To 175°C. This versatile silver conductive adhesive can be used for chip bonding in Micro and electronic hybrid circuit Fabrication. This unique conductive polymer also exhibits outstanding adhesion to a wide variety of substrates with good hot strength at intermittent temperatures up to 325°C. AA-DUCT N02 has also been used in microwave applications for EMI and FRI shielding, for assembly and repair of circuit boards and Electronic component manufacturing.

Appearance: Grey

Cure Type: Heat cure or Room temperature

Mix Ratio by weight: 100:6/Resin:Hardener

Benefits:

  • High strength
  • Perfect bond
  • Cold solder for heat sensitive components
  • Wave guides
Substrates: Excellent choice for Integrated Circuits, aluminum, copper, magnesium, steel, bronze, nickel, kovar, ceramic, glass, phenolic and G-10 epoxy glass boards.

Typical Application: Microwave applications for EMI and FRI shielding, for assembly and repair of circuit boards and Electronic component manufacturing.

Information provided by Atom Adhesives

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Outgassing - Total Mass Loss 0.070 %0.070 %WVR
 0.25 %0.25 %TTML
Collected Volatile Condensable Material 0.00 %0.00 %
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8888cured
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 0.038 ohm-cm0.038 ohm-cmcured
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity 1.46 W/m-K10.1 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 175 °C347 °F
Minimum Service Temperature, Air -55.0 °C-67.0 °F
 
Processing PropertiesMetricEnglishComments
Cure Time  30.0 min
@Temperature 175 °C
0.500 hour
@Temperature 347 °F
 60.0 min
@Temperature 150 °C
1.00 hour
@Temperature 302 °F
 120 min
@Temperature 125 °C
2.00 hour
@Temperature 257 °F
Shelf Life 6.00 Month6.00 Month
 
Descriptive Properties
ViscositySoft paste

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Atom Adhesives AA-BOND F253 Epoxy Adhesive
Atom Adhesives AA-CARB 61 Epoxy Adhesive
Atom Adhesives AA-DUCT 2979 Epoxy Adhesive
Atom Adhesives AA-DUCT 902LP Epoxy Adhesive
Atom Adhesives AA-SUPERTHERM 195 Epoxy Adhesive

PATOM050 / 172365

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.