MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ohara S-TIL 6 Optical Glass
Categories: Ceramic; Glass; Optical

Material Notes: ECO optical glass that does not contain any lead or arsenic.

Information provided by Ohara Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 2.50 g/cc2.50 g/cc
 
Chemical PropertiesMetricEnglishComments
Acid Class, SR 1.01.0
 
Mechanical PropertiesMetricEnglishComments
Hardness, Knoop 490
@Load 0.0999 kg
490
@Load 0.220 lb
Modulus of Elasticity 64.8 GPa9400 ksi
Modulus of Rigidity 28.3 GPa4100 ksi
Poissons Ratio 0.1460.146
Abrasion 114114Aa
 
Thermal PropertiesMetricEnglishComments
CTE, linear  8.20 µm/m-°C
@Temperature -30.0 - 70.0 °C
4.56 µin/in-°F
@Temperature -22.0 - 158 °F
 9.60 µm/m-°C
@Temperature 100 - 300 °C
5.33 µin/in-°F
@Temperature 212 - 572 °F
Thermal Conductivity 1.059 W/m-K
@Temperature 35.0 °C
7.349 BTU-in/hr-ft²-°F
@Temperature 95.0 °F
Transformation Temperature, Tg 479 °C894 °Fper thermal expansion curve
Softening Point 648 °C1200 °F107.65 poise; JIS-R3104 and ASTM-C338
Annealing Point 468 °C874 °F1013 poise; ASTM-C336
Strain Point 438 °C820 °F1014.5 poise; JIS-R3103 and ASTM-C336
 
Optical PropertiesMetricEnglishComments
Refractive Index  1.50292
@Wavelength 2325.42 nm
1.50292
@Wavelength 2325.42 nm
 1.50797
@Wavelength 1970.09 nm
1.50797
@Wavelength 1970.09 nm
 1.51342
@Wavelength 1529.58 nm
1.51342
@Wavelength 1529.58 nm
 1.51829
@Wavelength 1128.64 nm
1.51829
@Wavelength 1128.64 nm
 1.51993
@Wavelength 1013.98 nm
1.51993
@Wavelength 1013.98 nm
nt (Hg t line)
 1.52280
@Wavelength 852.11 nm
1.52280
@Wavelength 852.11 nm
ns (Cs s line)
 1.52479
@Wavelength 768.19 nm
1.52479
@Wavelength 768.19 nm
nA' (K A' line)
 1.52662
@Wavelength 706.52 nm
1.52662
@Wavelength 706.52 nm
nr (He r line)
 1.52846
@Wavelength 656.27 nm
1.52846
@Wavelength 656.27 nm
nC (H C line)
 1.52897
@Wavelength 643.85 nm
1.52897
@Wavelength 643.85 nm
nC' (Cd C' line)
 1.52946
@Wavelength 632.8 nm
1.52946
@Wavelength 632.8 nm
nHe-Ne
 1.53162
@Wavelength 589.29 nm
1.53162
@Wavelength 589.29 nm
nD (Na D line)
 1.53172
@Wavelength 587.56 nm
1.53172
@Wavelength 587.56 nm
nd (He D line)
 1.53430
@Wavelength 546.07 nm
1.53430
@Wavelength 546.07 nm
ne (Hg e line)
 1.53934
@Wavelength 486.13 nm
1.53934
@Wavelength 486.13 nm
nf (H F line)
 1.53998
@Wavelength 479.99 nm
1.53998
@Wavelength 479.99 nm
nF' (Cd F' line)
 1.54465
@Wavelength 441.57 nm
1.54465
@Wavelength 441.57 nm
nHe-Cd
 1.54547
@Wavelength 435.835 nm
1.54547
@Wavelength 435.835 nm
ng (Hg g line)
 1.55069
@Wavelength 404.656 nm
1.55069
@Wavelength 404.656 nm
nh (Hg h line)
 1.55989
@Wavelength 365.015 nm
1.55989
@Wavelength 365.015 nm
ni (Hg i line)
Abbe Number 48.5548.55ν e
 48.8448.84ν d
Optical Dispersion 0.0032610.003261nd-nC; Partial Dispersion
 0.0036670.003667nC-nA'; Partial Dispersion
 0.0052160.005216nh-ng; Partial Dispersion
 0.0053320.005332ne-nC'; Partial Dispersion
 0.0056740.005674nF'-ne; Partial Dispersion
 0.0058480.005848ne-nC; Partial Dispersion
 0.006130.00613ng-nF; Partial Dispersion
 0.0085290.008529nC-nt; Partial Dispersion
 0.0090450.009045nC'-nt; Partial Dispersion
 0.0108870.010887nF-nC
 0.0110060.011006nF'-nC'
 0.0137560.013756ng-nd; Partial Dispersion
 0.0144180.014418ni-ng; Partial Dispersion
 0.0199130.019913ni-nF'; Partial Dispersion
Transmission, Visible  94.8 %
@Wavelength 380 nm
94.8 %
@Wavelength 380 nm
 97.3 %
@Wavelength 390 nm
97.3 %
@Wavelength 390 nm
 98.5 %
@Wavelength 400 nm
98.5 %
@Wavelength 400 nm
 98.9 %
@Wavelength 440 nm
98.9 %
@Wavelength 440 nm
 99 %
@Wavelength 420 nm
99 %
@Wavelength 420 nm
 99 %
@Wavelength 460 nm
99 %
@Wavelength 460 nm
 99.1 %
@Wavelength 480 nm
99.1 %
@Wavelength 480 nm
 99.2 %
@Wavelength 650 nm
99.2 %
@Wavelength 650 nm
 99.3 %
@Wavelength 500 nm
99.3 %
@Wavelength 500 nm
 99.4 %
@Wavelength 550 nm
99.4 %
@Wavelength 550 nm
 99.4 %
@Wavelength 600 nm
99.4 %
@Wavelength 600 nm
 99.6 %
@Wavelength 700 nm
99.6 %
@Wavelength 700 nm
IR Transmittance  85 %
@Wavelength 2400 nm
85 %
@Wavelength 2400 nm
 89 %
@Wavelength 2200 nm
89 %
@Wavelength 2200 nm
 97.7 %
@Wavelength 1800 nm
97.7 %
@Wavelength 1800 nm
 99.3 %
@Wavelength 1600 nm
99.3 %
@Wavelength 1600 nm
 99.5 %
@Wavelength 1400 nm
99.5 %
@Wavelength 1400 nm
 99.6 %
@Wavelength 1200 nm
99.6 %
@Wavelength 1200 nm
 99.7 %
@Wavelength 900 nm
99.7 %
@Wavelength 900 nm
 99.7 %
@Wavelength 1000 nm
99.7 %
@Wavelength 1000 nm
 99.8 %
@Wavelength 800 nm
99.8 %
@Wavelength 800 nm
UV Transmittance  7.0 %
@Wavelength 340 nm
7.0 %
@Wavelength 340 nm
 44 %
@Wavelength 350 nm
44 %
@Wavelength 350 nm
 74 %
@Wavelength 360 nm
74 %
@Wavelength 360 nm
 88 %
@Wavelength 370 nm
88 %
@Wavelength 370 nm
 
Descriptive Properties
Acid Resistance, Powder Method, RAP)1
Bubble GroupB
CCI0.00 B
 0.28 G
 0.28 R
coloring, λ 5335
coloring, λ 80365
Coloring, Internal Transmission λ 0.05339
Coloring, Internal Transmission λ 0.80364
Knoop Hardness Class5
Melt Frequency1
Ohara Code d532489
Ohara Code e534485
Ohara StatusPreferred
Phosphate Resistance, PR1
Photoelastic Constant (ß)2.81
Relative Price4S-BSL7 = 1
Water Resistance, RW(P)3
Weathering Resistance (Surface Method) W(S)max2
Weathering Resistance (Surface Method) W(S)min3
Yield Point, At (°C)528per thermal expansion curve

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Schott N-PK51 Glass
Schott N-KZFS11 638424.320, Optical Glass
Ohara S-TIH53 Optical Glass
Ohara S-TIH11 Optical Glass
Ohara S-PHM52 Optical Glass

CZOHARA952 / 192217

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.