MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Kennametal Stellite Stellite® 3 PM with P/M Processing
Categories: Metal; Nonferrous Metal; Cobalt Alloy; Superalloy

Material Notes: Typical applications include (aerospace) vane plugs, fuel metering pins, spacer bushings, (bearings) ball blanks, race blanks, (valve seat inserts) diesel engine exhaust, fluid valve seats, saw cutter inserts, miscellaneous wear parts. Adhesive wear test data: P/M 0.10, Cast 0.24. Data provided by the manufacturer, Deloro Stellite Inc.

Product of former Deloro Stellite Inc.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.40 g/cc0.303 lb/in³P/M (97%); 8.64 g/cc theoretical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 533533Converted from Rockwell C hardness.
 271
@Temperature 760 °C
271
@Temperature 1400 °F
Converted from Rockwell C hardness
 354
@Temperature 649 °C
354
@Temperature 1200 °F
Converted from Rockwell C hardness
 427
@Temperature 538 °C
427
@Temperature 1000 °F
Converted from Rockwell C hardness
Hardness, Knoop 643643Converted from Rockwell C hardness.
 321
@Temperature 760 °C
321
@Temperature 1400 °F
Converted from Rockwell C hardness
 424
@Temperature 649 °C
424
@Temperature 1200 °F
Converted from Rockwell C hardness
 513
@Temperature 538 °C
513
@Temperature 1000 °F
Converted from Rockwell C hardness
Hardness, Rockwell A 7777Converted from Rockwell C hardness.
 64
@Temperature 760 °C
64
@Temperature 1400 °F
Converted from Rockwell C hardness
 70
@Temperature 649 °C
70
@Temperature 1200 °F
Converted from Rockwell C hardness
 73
@Temperature 538 °C
73
@Temperature 1000 °F
Converted from Rockwell C hardness
Hardness, Rockwell C 5454Hot hardness.
 28
@Temperature 760 °C
28
@Temperature 1400 °F
Hot hardness.
 39
@Temperature 649 °C
39
@Temperature 1200 °F
Hot hardness.
 46
@Temperature 538 °C
46
@Temperature 1000 °F
Hot hardness.
Hardness, Vickers 575575Converted from Rockwell C hardness.
 280
@Temperature 760 °C
280
@Temperature 1400 °F
Converted from Rockwell C hardness
 372
@Temperature 649 °C
372
@Temperature 1200 °F
Converted from Rockwell C hardness
 454
@Temperature 538 °C
454
@Temperature 1000 °F
Converted from Rockwell C hardness
Tensile Strength, Ultimate 863 MPa125000 psi
 621 MPa
@Temperature 760 °C
90100 psi
@Temperature 1400 °F
 690 MPa
@Temperature 649 °C
100000 psi
@Temperature 1200 °F
 725 MPa
@Temperature 538 °C
105000 psi
@Temperature 1000 °F
Elongation at Break <= 1.0 %<= 1.0 %in 25.4 mm
 
Electrical PropertiesMetricEnglishComments
Magnetic Permeability <= 1.2
@Temperature 22.0 °C
<= 1.2
@Temperature 71.6 °F
200 Oersted
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.3 µm/m-°C
@Temperature 0.000 - 100 °C
6.83 µin/in-°F
@Temperature 32.0 - 212 °F
 12.5 µm/m-°C
@Temperature 0.000 - 200 °C
6.94 µin/in-°F
@Temperature 32.0 - 392 °F
 12.7 µm/m-°C
@Temperature 0.000 - 300 °C
7.06 µin/in-°F
@Temperature 32.0 - 572 °F
 12.9 µm/m-°C
@Temperature 0.000 - 400 °C
7.17 µin/in-°F
@Temperature 32.0 - 752 °F
 13.0 µm/m-°C
@Temperature 0.000 - 500 °C
7.22 µin/in-°F
@Temperature 32.0 - 932 °F
 13.1 µm/m-°C
@Temperature 0.000 - 600 °C
7.28 µin/in-°F
@Temperature 32.0 - 1110 °F
 13.4 µm/m-°C
@Temperature 0.000 - 700 °C
7.44 µin/in-°F
@Temperature 32.0 - 1290 °F
 13.7 µm/m-°C
@Temperature 0.000 - 800 °C
7.61 µin/in-°F
@Temperature 32.0 - 1470 °F
 14.5 µm/m-°C
@Temperature 0.000 - 900 °C
8.06 µin/in-°F
@Temperature 32.0 - 1650 °F
 16.0 µm/m-°C
@Temperature 0.000 - 1000 °C
8.89 µin/in-°F
@Temperature 32.0 - 1830 °F
Melting Point 1213 - 1285 °C2215 - 2345 °F
Solidus 1213 °C2215 °F
Liquidus 1285 °C2345 °F
 
Component Elements PropertiesMetricEnglishComments
Boron, B <= 1.0 %<= 1.0 %
Carbon, C 2.4 %2.4 %
Chromium, Cr 31 %31 %
Cobalt, Co 44 %44 %As remainder
Iron, Fe <= 3.0 %<= 3.0 %
Manganese, Mn <= 1.0 %<= 1.0 %
Nickel, Ni <= 3.0 %<= 3.0 %
Other <= 1.0 %<= 1.0 %
Silicon, Si <= 1.0 %<= 1.0 %
Tungsten, W 12.5 %12.5 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Kennametal Stellite Stellite® 6 PM with P/M Processing
Kennametal Stellite Stellite® 6 PM cast
Kennametal Stellite Stellite® 3 PM cast
Kennametal Stellite Stellite® 12 PM with P/M Processing
Kennametal Stellite Nucalloy® 41 Nickel-Chromium-Boron Alloy

NS3PMA / 18871

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.