MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Adell AD-30 Nylon 66, Ultra High Impact
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Impact Grade

Material Notes: Data provided by Adell Plastics, Inc.

Key Words: Polyamide 66; Nylon 6,6; Adell Plastics, Inc.; Adell Nylon 6/6; Polyamide 6/6
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.08 g/cc0.0390 lb/in³ASTM D792
Water Absorption 1.2 %1.2 %24 hour immersion; ASTM D570
Linear Mold Shrinkage 0.0145 cm/cm0.0145 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 6464ASTM D785
Hardness, Rockwell R 111111ASTM D785
Tensile Strength, Ultimate 52.4 MPa7600 psiASTM D638
Elongation at Break 65 %65 %ASTM D638
Flexural Strength 72.0 MPa10400 psiASTM D790
Flexural Modulus 1.80 GPa261 ksiASTM D790
Compressive Yield Strength 66.0 MPa9570 psiASTM D695
Izod Impact, Notched 8.50 J/cm15.9 ft-lb/inASTM D256
 
Thermal PropertiesMetricEnglishComments
Melting Point 255 °C491 °FASTM D789
Deflection Temperature at 0.46 MPa (66 psi) 216 °C421 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 70.0 °C158 °FASTM D648
Flammability, UL94 HBHB

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Clariant Renol PA121 Nylon 66, Impact Modified
Overview of materials for Nylon 66, Impact Grade
BASF Ultramid® A3L HP BK20465 PA66 (Conditioned)
Chase Plastics CP Pryme® NN200STL (COND, 50% RH) Nylon 66, Super-Toughened, Internally Lubricated
Celanese Zytel® ST801AHS BK010 PA66-HI

PDEL41 / 29602

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.