Physical Properties | Metric | English | Comments |
---|
Density | 1.37 g/cc | 0.0495 lb/in³ |
Water Absorption | 0.80 % @Temperature 23.0 °C, Time 86400 sec | 0.80 % @Temperature 73.4 °F, Time 24.0 hour |
Viscosity | 20 cP @Shear Rate 1000 1/s, Temperature 280 °C | 20 cP @Shear Rate 1000 1/s, Temperature 536 °F |
| 20 cP @Shear Rate 1000 1/s, Temperature 290 °C | 20 cP @Shear Rate 1000 1/s, Temperature 554 °F |
| 20 cP @Shear Rate 1000 1/s, Temperature 300 °C | 20 cP @Shear Rate 1000 1/s, Temperature 572 °F |
| 120 cP @Shear Rate 10 1/s, Temperature 300 °C | 120 cP @Shear Rate 10 1/s, Temperature 572 °F |
| 135 cP @Shear Rate 100 1/s, Temperature 300 °C | 135 cP @Shear Rate 100 1/s, Temperature 572 °F |
| 140 cP @Shear Rate 100 1/s, Temperature 290 °C | 140 cP @Shear Rate 100 1/s, Temperature 554 °F |
| 150 cP @Shear Rate 100 1/s, Temperature 280 °C | 150 cP @Shear Rate 100 1/s, Temperature 536 °F |
| 250 cP @Shear Rate 10 1/s, Temperature 290 °C | 250 cP @Shear Rate 10 1/s, Temperature 554 °F |
| 300 cP @Shear Rate 10 1/s, Temperature 280 °C | 300 cP @Shear Rate 10 1/s, Temperature 536 °F |
Linear Mold Shrinkage | 0.0062 cm/cm | 0.0062 in/in |
Linear Mold Shrinkage, Flow | 0.0050 cm/cm | 0.0050 in/in |
Linear Mold Shrinkage, Transverse | 0.0080 cm/cm | 0.0080 in/in |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength at Break | 190 MPa | 27600 psi |
Tensile Stress at Strain | 30.0 MPa @Strain 1 %, Temperature 120 °C | 4350 psi @Strain 1 %, Temperature 248 °F |
| 40.0 MPa @Strain 1 %, Temperature 100 °C | 5800 psi @Strain 1 %, Temperature 212 °F |
| 45.0 MPa @Strain 1 %, Temperature 80.0 °C | 6530 psi @Strain 1 %, Temperature 176 °F |
| 60.0 MPa @Strain 2 %, Temperature 0.000 °C | 8700 psi @Strain 2 %, Temperature 32.0 °F |
| 65.0 MPa @Strain 2 %, Temperature 120 °C | 9430 psi @Strain 2 %, Temperature 248 °F |
| 70.0 MPa @Strain 2 %, Temperature 100 °C | 10200 psi @Strain 2 %, Temperature 212 °F |
| 80.0 MPa @Strain 2 %, Temperature 80.0 °C | 11600 psi @Strain 2 %, Temperature 176 °F |
| 80.0 MPa @Strain 3 %, Temperature 120 °C | 11600 psi @Strain 3 %, Temperature 248 °F |
| 90.0 MPa @Strain 1 %, Temperature -30.0 °C | 13100 psi @Strain 1 %, Temperature -22.0 °F |
| 90.0 MPa @Strain 1 %, Temperature 0.000 °C | 13100 psi @Strain 1 %, Temperature 32.0 °F |
| 90.0 MPa @Strain 1 %, Temperature 23.0 °C | 13100 psi @Strain 1 %, Temperature 73.4 °F |
| 90.0 MPa @Strain 3 %, Temperature 100 °C | 13100 psi @Strain 3 %, Temperature 212 °F |
| 90.0 MPa @Strain 4 %, Temperature 120 °C | 13100 psi @Strain 4 %, Temperature 248 °F |
| 100 MPa @Strain 3 %, Temperature 80.0 °C | 14500 psi @Strain 3 %, Temperature 176 °F |
| 100 MPa @Strain 4 %, Temperature 100 °C | 14500 psi @Strain 4 %, Temperature 212 °F |
| 100 MPa @Strain 6.0 %, Temperature 120 °C | 14500 psi @Strain 6.0 %, Temperature 248 °F |
| 102 MPa @Strain 9.0 %, Temperature 120 °C | 14800 psi @Strain 9.0 %, Temperature 248 °F |
| 110 MPa @Strain 6.0 %, Temperature 100 °C | 16000 psi @Strain 6.0 %, Temperature 212 °F |
| 110 MPa @Strain 9.0 %, Temperature 100 °C | 16000 psi @Strain 9.0 %, Temperature 212 °F |
| 115 MPa @Strain 4 %, Temperature 80.0 °C | 16700 psi @Strain 4 %, Temperature 176 °F |
| 120 MPa @Strain 6.0 %, Temperature 80.0 °C | 17400 psi @Strain 6.0 %, Temperature 176 °F |
| 160 MPa @Strain 2 %, Temperature 23.0 °C | 23200 psi @Strain 2 %, Temperature 73.4 °F |
| 170 MPa @Strain 2 %, Temperature -30.0 °C | 24700 psi @Strain 2 %, Temperature -22.0 °F |
| 190 MPa @Strain 3 %, Temperature 0.000 °C | 27600 psi @Strain 3 %, Temperature 32.0 °F |
| 195 MPa @Strain 3 %, Temperature 23.0 °C | 28300 psi @Strain 3 %, Temperature 73.4 °F |
| 210 MPa @Strain 3 %, Temperature -30.0 °C | 30500 psi @Strain 3 %, Temperature -22.0 °F |
Elongation at Break | 3.0 % | 3.0 % |
Tensile Modulus | 10.0 GPa | 1450 ksi |
Flexural Strength | 280 MPa | 40600 psi |
| 290 MPa | 42100 psi |
Flexural Modulus | 9.00 GPa | 1310 ksi |
Izod Impact, Notched | 1.15 J/cm | 2.15 ft-lb/in |
Izod Impact, Unnotched (ISO) | 60.0 kJ/m² | 28.6 ft-lb/in² |
Charpy Impact Unnotched | 8.00 J/cm² | 38.1 ft-lb/in² |
Charpy Impact, Notched | 1.10 J/cm² | 5.23 ft-lb/in² |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | 1.00e+15 ohm-cm | 1.00e+15 ohm-cm |
Surface Resistance | 6.00e+14 ohm | 6.00e+14 ohm |
Dielectric Constant | 3.7 | 3.7 |
Dielectric Strength | 34.0 kV/mm | 864 kV/in |
Dissipation Factor | 0.010 | 0.010 |
Comparative Tracking Index | 500 V | 500 V |
| 600 V | 600 V |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear, Parallel to Flow | 25.0 µm/m-°C @Temperature 23.0 - 85.0 °C | 13.9 µin/in-°F @Temperature 73.4 - 185 °F |
CTE, linear, Transverse to Flow | 25.0 µm/m-°C @Temperature 23.0 - 85.0 °C | 13.9 µin/in-°F @Temperature 73.4 - 185 °F |
Melting Point | 260 °C | 500 °F |
| 263 °C | 505 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 255 °C | 491 °F |
Flammability, UL94 | HB @Thickness 1.60 mm | HB @Thickness 0.0630 in |
Oxygen Index | 23 % | 23 % |
Glow Wire Flammability Index | 700 °C @Thickness 1.60 mm | 1290 °F @Thickness 0.0630 in |
|
Processing Properties | Metric | English | Comments |
---|
Feed Temperature | 265 - 275 °C | 509 - 527 °F |
Mold Temperature | 70.0 - 100 °C | 158 - 212 °F |
Drying Temperature | 80.0 °C | 176 °F |
Moisture Content | <= 0.20 % | <= 0.20 % |
|
Descriptive Properties |
---|
Compression Zone | 270-280°C |
Mixing Zone | 280-290°C |