MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Dow ATTANE™ 4404G, 2mil Ultra Low Density Ethylene/Octene Copolymer
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Low Density (LDPE)

Material Notes: ATTANE™ 4201G provides improved cling in one-sided cling applications, and has improved toughness and optical properties. It complies with U.S. FDA 21 CFR 177.1520 (c) 3.2a.

Information provided by Dow

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.904 g/cc0.0327 lb/in³ASTM D792
Water Vapor Transmission 16.7 g/m²/day
@Pressure 0.101 MPa,
Temperature 38.0 °C
1.08 g/100 in²/day
@Pressure 14.7 psi,
Temperature 100 °F
100% RH; ASTM D1249
Oxygen Transmission 445.7 cc-mm/m²-24hr-atm1132 cc-mil/100 in²-24hr-atmASTM D3985
Carbon Dioxide Transmission 2022 cc-mm/m²-24hr-atm5136 cc-mil/100 in²-24hr-atmDow Method
Thickness 50.8 microns2.00 mil
Melt Flow 4.0 g/10 min4.0 g/10 minASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 6.76 MPa980 psiASTM D882
Film Tensile Strength at Yield, TD 6.34 MPa919 psiASTM D882
Film Elongation at Break, MD 664 %664 %ASTM D882
Film Elongation at Break, TD 714 %714 %ASTM D882
Secant Modulus, MD 0.062563 GPa9.0741 ksi2% Secant; ASTM D882
Secant Modulus, TD 0.06298 GPa9.135 ksi2% Secant; ASTM D882
Impact 211211[ft-lbf/in3]; Puncture Resistance; Dow Method
Elmendorf Tear Strength MD 955 g955 gASTM D1922
Elmendorf Tear Strength TD 1100 g1100 gASTM D1922
Elmendorf Tear Strength, MD 18.80 g/micron477.5 g/milASTM D1922
Elmendorf Tear Strength, TD 21.7 g/micron550 g/milASTM D1922
Dart Drop Test >= 850 g>= 1.87 lbMethod B; ASTM D1709
Film Tensile Strength at Break, MD 32.60 MPa4728 psiASTM D882
Film Tensile Strength at Break, TD 32.43 MPa4703 psiASTM D882
 
Thermal PropertiesMetricEnglishComments
Melting Point 124 °C255 °FDow Method (DSC)
Vicat Softening Point 71.0 °C160 °FASTM D1525
 
Optical PropertiesMetricEnglishComments
Haze 1.8 %1.8 %ASTM D1003
Gloss 90 %90 %45°; ASTM D2457
Transmission, Visible 99 %99 %Clarity; ASTM D1746
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Dow ATTANE™ 4404G, 0.8mil Ultra Low Density Ethylene/Octene Copolymer
Dow ATTANE™ 4401 Ultra Low Density Polyethylene, Blown Film Grade
Dow ATTANE™ 4202 Ultra Low Density Polyethylene, Cast Film Grade
Dow ATTANE™ 4201G, 2mil Ultra Low Density Ethylene/Octene Copolymer
Dow ATTANE™ 4402 Ultra Low Density Polyethylene, Cast Film Grade

PDOW1196 / 30414

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.