MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Tisan TISLAMID® 6 30% Glass Filled Impact Modified Nylon 6
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Glass Filled, Impact Grade

Material Notes: TISLAMID has a wide area of application in electric/electronic, automotive, durable goods and telecommunications industries. It demonstrates characteristics such as
  • Excellent chemical resistance
  • Electric isolation
  • Easy processability
  • High mechanical resistance
  • Excellent flame retardance
  • High moisture absorption
  • Excellent temperature resistance
  • High performance / affordable price
  • Abrasion resistance
TISLAMID has an excellent resistance to weak alkalis and organic solvents. It has a good resistance to weak acids, alcohols, hydrocarbons, and engine fuels. It has a medium resistance to strong alkalis and a weak resistance to strong acids.

Key Words: PA 6
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.33 g/cc0.0480 lb/in³ISO 1183
Moisture Absorption 1.8 %1.8 %ISO 62
Linear Mold Shrinkage 0.0030 cm/cm0.0030 in/in
Ash 30 %30 %ISO 3451
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 99.0 MPa14400 psiISO 527-2
Tensile Strength, Yield 100 MPa14500 psiISO 527-2
Elongation at Break 4.5 %4.5 %ISO 527-2
Elongation at Yield 4.0 %4.0 %ISO 527-2
Modulus of Elasticity 6.50 GPa943 ksiISO 527-2
Izod Impact, Notched (ISO) 19.0 kJ/m²9.04 ft-lb/in²ISO 180
 
Electrical PropertiesMetricEnglishComments
Comparative Tracking Index 500 V500 VTS EN 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 220 - 225 °C428 - 437 °F
Vicat Softening Point 200 °C392 °FISO 306
Heat Distortion Temperature 215 °C419 °FISO 75-2
Flammability, UL94 HBHB
Glow Wire Test 650 °C1200 °F60695-2-10
 
Processing PropertiesMetricEnglishComments
Feed Temperature 60.0 - 80.0 °C140 - 176 °F
Rear Barrel Temperature 220 - 240 °C428 - 464 °FAft-1. Region Temperature
Middle Barrel Temperature 220 - 240 °C428 - 464 °FMid-2. Region Temperature
Front Barrel Temperature 220 - 240 °C428 - 464 °FPre-3. Region Temperature
Nozzle Temperature 210 - 230 °C410 - 446 °F
Melt Temperature 220 - 240 °C428 - 464 °F
Drying Temperature 90.0 - 100 °C194 - 212 °FPredrying Temperature
Dry Time 3 - 4 hour3 - 4 hourPredrying Time
 
Descriptive Properties
Block Temperature60-80°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Tisan TISLAMID® 66 30% Glass Filled Impact Modified, Heat Stabilized Nylon 66
Tisan TISLAMID® 6 30% Glass Fiber Reinforced Nylon 6
BASF Ultramid® B3WG6 30% Glass Filled PA6 (Conditioned)

PTIS006 / 79441

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.