MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Kennametal Stellite Deloro® 711 PM after P/M Processing
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Adhesive wear test data: P/M 0.1, cast 0.1; Abrasive wear test data P/M 6 mm^3, cast 26 mm^3. Typical applications include vane plugs, fuel metering pins, spacer bushings, ball bearing blanks, race bearing blanks, diesel engine exhaust, fluid valve seats, saw cutter inserts, miscellaneous wear parts. Data provided by the manufacturer, Deloro Stellite Inc.

Product of former Deloro Stellite Inc.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.00 g/cc0.289 lb/in³theoretical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 476476Converted from Rockwell C hardness.
 394
@Temperature 538 °C
394
@Temperature 1000 °F
Converted from Rockwell C hardness
 394
@Temperature 649 °C
394
@Temperature 1200 °F
Converted from Rockwell C hardness
Hardness, Knoop 574574Converted from Rockwell C hardness.
 473
@Temperature 538 °C
473
@Temperature 1000 °F
Converted from Rockwell C hardness
 473
@Temperature 649 °C
473
@Temperature 1200 °F
Converted from Rockwell C hardness
Hardness, Rockwell A 7575Converted from Rockwell C hardness.
 72
@Temperature 538 °C
72
@Temperature 1000 °F
Converted from Rockwell C hardness
 72
@Temperature 649 °C
72
@Temperature 1200 °F
Converted from Rockwell C hardness
Hardness, Rockwell C 5050Hot hardness.
 43
@Temperature 538 °C
43
@Temperature 1000 °F
Hot hardness.
 43
@Temperature 649 °C
43
@Temperature 1200 °F
Hot hardness.
Hardness, Vickers 510510Converted from Rockwell C hardness.
 416
@Temperature 538 °C
416
@Temperature 1000 °F
Converted from Rockwell C hardness
 416
@Temperature 649 °C
416
@Temperature 1200 °F
Converted from Rockwell C hardness
Tensile Strength, Ultimate 559 MPa81100 psi
 490 MPa
@Temperature 538 °C
71100 psi
@Temperature 1000 °F
 490 MPa
@Temperature 649 °C
71100 psi
@Temperature 1200 °F
 504 MPa
@Temperature 760 °C
73100 psi
@Temperature 1400 °F
Elongation at Break <= 1.0 %<= 1.0 %in 25.4 mm
 <= 1.0 %
@Temperature 538 °C
<= 1.0 %
@Temperature 1000 °F
in 25.4 mm
 <= 1.0 %
@Temperature 649 °C
<= 1.0 %
@Temperature 1200 °F
in 25.4 mm
 
Component Elements PropertiesMetricEnglishComments
Boron, B <= 1.0 %<= 1.0 %
Carbon, C 2.7 %2.7 %
Chromium, Cr 27 %27 %
Cobalt, Co 12 %12 %
Iron, Fe 23 %23 %
Molybdenum, Mo 7.0 %7.0 %
Nickel, Ni 23 %23 %as balance
Tungsten, W 3.0 %3.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Kennametal Stellite Deloro® N-6 PM with P/M Processing
Kennametal Stellite Deloro® 208 PM after P/M Processing
Kennametal Stellite Deloro® 40G
Kennametal Stellite Deloro® 711 PM cast
Kennametal Stellite Deloro® 716 PM with P/M Processing

ND711A / 16083

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.