Physical Properties | Metric | English | Comments |
---|
Density | 8.20 g/cc | 0.296 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell C | 40.9 @Thickness 44.5 mm | 40.9 @Thickness 1.75 in |
| 41 @Thickness 17.7 mm | 41 @Thickness 0.697 in |
| 41 @Thickness 22.5 mm | 41 @Thickness 0.886 in |
| 42 @Thickness 30.6 mm | 42 @Thickness 1.20 in |
Tensile Strength | 1156 MPa @Diameter 17.7 mm | 167700 psi @Diameter 0.697 in |
| 1346 MPa @Diameter 44.5 mm | 195200 psi @Diameter 1.75 in |
| 1355 MPa @Diameter 30.6 mm | 196500 psi @Diameter 1.20 in |
| 1455 MPa @Diameter 22.5 mm | 211000 psi @Diameter 0.886 in |
Tensile Strength, Yield | 1178 MPa @Thickness 17.7 mm | 170900 psi @Thickness 0.697 in |
| 1180 MPa @Thickness 22.5 mm | 171000 psi @Thickness 0.886 in |
| 1206 MPa @Thickness 30.6 mm | 174900 psi @Thickness 1.20 in |
| 1218 MPa @Thickness 44.5 mm | 176700 psi @Thickness 1.75 in |
Elongation at Break | 15.6 % @Diameter 30.6 mm | 15.6 % @Diameter 1.20 in |
| 16.3 % @Diameter 22.5 mm | 16.3 % @Diameter 0.886 in |
| 17 % @Diameter 44.5 mm | 17 % @Diameter 1.75 in |
| 17.1 % @Diameter 17.7 mm | 17.1 % @Diameter 0.697 in |
Reduction of Area | 26.3 % @Diameter 30.6 mm | 26.3 % @Diameter 1.20 in |
| 26.6 % @Diameter 17.7 mm | 26.6 % @Diameter 0.697 in |
| 27.3 % @Diameter 22.5 mm | 27.3 % @Diameter 0.886 in |
| 29.2 % @Diameter 44.5 mm | 29.2 % @Diameter 1.75 in |
Modulus of Elasticity | 155 GPa @Temperature 704 °C | 22500 ksi @Temperature 1300 °F |
| 159 GPa @Temperature 649 °C | 23100 ksi @Temperature 1200 °F |
| 163 GPa @Temperature 593 °C | 23600 ksi @Temperature 1100 °F |
| 167 GPa @Temperature 538 °C | 24200 ksi @Temperature 1000 °F |
| 169 GPa @Temperature 482 °C | 24500 ksi @Temperature 900 °F |
| 173 GPa @Temperature 427 °C | 25100 ksi @Temperature 801 °F |
| 176 GPa @Temperature 371 °C | 25500 ksi @Temperature 700 °F |
| 179 GPa @Temperature 316 °C | 26000 ksi @Temperature 601 °F |
| 182 GPa @Temperature 260 °C | 26400 ksi @Temperature 500 °F |
| 185 GPa @Temperature 204 °C | 26800 ksi @Temperature 399 °F |
| 188 GPa @Temperature 149 °C | 27300 ksi @Temperature 300 °F |
| 192 GPa @Temperature 93.0 °C | 27800 ksi @Temperature 199 °F |
| 195 GPa @Temperature 23.0 °C | 28300 ksi @Temperature 73.4 °F |
Poissons Ratio | 0.31 @Temperature 23.0 °C | 0.31 @Temperature 73.4 °F |
| 0.31 @Temperature 93.0 °C | 0.31 @Temperature 199 °F |
| 0.31 @Temperature 149 °C | 0.31 @Temperature 300 °F |
| 0.31 @Temperature 204 °C | 0.31 @Temperature 399 °F |
| 0.32 @Temperature 260 °C | 0.32 @Temperature 500 °F |
| 0.32 @Temperature 316 °C | 0.32 @Temperature 601 °F |
| 0.32 @Temperature 371 °C | 0.32 @Temperature 700 °F |
| 0.32 @Temperature 427 °C | 0.32 @Temperature 801 °F |
| 0.32 @Temperature 482 °C | 0.32 @Temperature 900 °F |
| 0.33 @Temperature 538 °C | 0.33 @Temperature 1000 °F |
| 0.33 @Temperature 593 °C | 0.33 @Temperature 1100 °F |
| 0.34 @Temperature 649 °C | 0.34 @Temperature 1200 °F |
| 0.34 @Temperature 704 °C | 0.34 @Temperature 1300 °F |
Fatigue Strength | 414 MPa @Frequency 100 Hz, # of Cycles 1.00e+7 | 60000 psi @Frequency 100 Hz, # of Cycles 1.00e+7 |
| 517 MPa @Frequency 100 Hz, # of Cycles 1.00e+6 | 75000 psi @Frequency 100 Hz, # of Cycles 1.00e+6 |
| 552 MPa @Frequency 100 Hz, # of Cycles 300000 | 80000 psi @Frequency 100 Hz, # of Cycles 300000 |
Shear Modulus | 58.0 GPa @Temperature 704 °C | 8410 ksi @Temperature 1300 °F |
| 59.0 GPa @Temperature 649 °C | 8560 ksi @Temperature 1200 °F |
| 61.0 GPa @Temperature 593 °C | 8850 ksi @Temperature 1100 °F |
| 63.0 GPa @Temperature 538 °C | 9140 ksi @Temperature 1000 °F |
| 64.0 GPa @Temperature 482 °C | 9280 ksi @Temperature 900 °F |
| 65.0 GPa @Temperature 427 °C | 9430 ksi @Temperature 801 °F |
| 67.0 GPa @Temperature 371 °C | 9720 ksi @Temperature 700 °F |
| 68.0 GPa @Temperature 316 °C | 9860 ksi @Temperature 601 °F |
| 69.0 GPa @Temperature 260 °C | 10000 ksi @Temperature 500 °F |
| 70.0 GPa @Temperature 149 °C | 10200 ksi @Temperature 300 °F |
| 70.0 GPa @Temperature 204 °C | 10200 ksi @Temperature 399 °F |
| 74.0 GPa @Temperature 23.0 °C | 10700 ksi @Temperature 73.4 °F |
| 74.0 GPa @Temperature 93.0 °C | 10700 ksi @Temperature 199 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.000110 ohm-cm | 0.000110 ohm-cm |
Magnetic Permeability | 1.003 | 1.003 |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 14.19 µm/m-°C @Temperature 25.0 - 93.0 °C | 7.883 µin/in-°F @Temperature 77.0 - 199 °F |
| 14.24 µm/m-°C @Temperature 25.0 - 149 °C | 7.911 µin/in-°F @Temperature 77.0 - 300 °F |
| 14.36 µm/m-°C @Temperature 25.0 - 204 °C | 7.978 µin/in-°F @Temperature 77.0 - 399 °F |
| 14.47 µm/m-°C @Temperature 25.0 - 260 °C | 8.039 µin/in-°F @Temperature 77.0 - 500 °F |
| 14.69 µm/m-°C @Temperature 25.0 - 316 °C | 8.161 µin/in-°F @Temperature 77.0 - 601 °F |
| 14.94 µm/m-°C @Temperature 25.0 - 371 °C | 8.300 µin/in-°F @Temperature 77.0 - 700 °F |
| 15.12 µm/m-°C @Temperature 25.0 - 427 °C | 8.400 µin/in-°F @Temperature 77.0 - 801 °F |
| 15.26 µm/m-°C @Temperature 25.0 - 482 °C | 8.478 µin/in-°F @Temperature 77.0 - 900 °F |
| 15.39 µm/m-°C @Temperature 25.0 - 538 °C | 8.550 µin/in-°F @Temperature 77.0 - 1000 °F |
| 15.64 µm/m-°C @Temperature 25.0 - 593 °C | 8.689 µin/in-°F @Temperature 77.0 - 1100 °F |
| 15.93 µm/m-°C @Temperature 25.0 - 649 °C | 8.850 µin/in-°F @Temperature 77.0 - 1200 °F |
| 16.32 µm/m-°C @Temperature 25.0 - 704 °C | 9.067 µin/in-°F @Temperature 77.0 - 1300 °F |
| 16.89 µm/m-°C @Temperature 25.0 - 760 °C | 9.383 µin/in-°F @Temperature 77.0 - 1400 °F |
| 17.47 µm/m-°C @Temperature 25.0 - 916 °C | 9.706 µin/in-°F @Temperature 77.0 - 1680 °F |
| 18.01 µm/m-°C @Temperature 25.0 - 871 °C | 10.01 µin/in-°F @Temperature 77.0 - 1600 °F |
Specific Heat Capacity | 0.445 J/g-°C @Temperature 23.0 °C | 0.106 BTU/lb-°F @Temperature 73.4 °F |
| 0.455 J/g-°C @Temperature 50.0 °C | 0.109 BTU/lb-°F @Temperature 122 °F |
| 0.467 J/g-°C @Temperature 100 °C | 0.112 BTU/lb-°F @Temperature 212 °F |
| 0.491 J/g-°C @Temperature 200 °C | 0.117 BTU/lb-°F @Temperature 392 °F |
| 0.515 J/g-°C @Temperature 300 °C | 0.123 BTU/lb-°F @Temperature 572 °F |
| 0.540 J/g-°C @Temperature 400 °C | 0.129 BTU/lb-°F @Temperature 752 °F |
| 0.563 J/g-°C @Temperature 500 °C | 0.135 BTU/lb-°F @Temperature 932 °F |
| 0.588 J/g-°C @Temperature 600 °C | 0.141 BTU/lb-°F @Temperature 1110 °F |
| 0.607 J/g-°C @Temperature 700 °C | 0.145 BTU/lb-°F @Temperature 1290 °F |
| 0.639 J/g-°C @Temperature 800 °C | 0.153 BTU/lb-°F @Temperature 1470 °F |
| 0.670 J/g-°C @Temperature 900 °C | 0.160 BTU/lb-°F @Temperature 1650 °F |
| 0.688 J/g-°C @Temperature 1000 °C | 0.164 BTU/lb-°F @Temperature 1830 °F |
| 0.690 J/g-°C @Temperature 1100 °C | 0.165 BTU/lb-°F @Temperature 2010 °F |
| 0.700 J/g-°C @Temperature 1150 °C | 0.167 BTU/lb-°F @Temperature 2100 °F |
Thermal Conductivity | 10.9 W/m-K @Temperature 23.0 °C | 75.6 BTU-in/hr-ft²-°F @Temperature 73.4 °F |
| 11.5 W/m-K @Temperature 50.0 °C | 79.8 BTU-in/hr-ft²-°F @Temperature 122 °F |
| 12.5 W/m-K @Temperature 100 °C | 86.8 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 14.4 W/m-K @Temperature 200 °C | 99.9 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 16.4 W/m-K @Temperature 300 °C | 114 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 18.4 W/m-K @Temperature 400 °C | 128 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 20.3 W/m-K @Temperature 500 °C | 141 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 22.4 W/m-K @Temperature 600 °C | 155 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 23.9 W/m-K @Temperature 700 °C | 166 BTU-in/hr-ft²-°F @Temperature 1290 °F |
| 25.7 W/m-K @Temperature 800 °C | 178 BTU-in/hr-ft²-°F @Temperature 1470 °F |
| 26.2 W/m-K @Temperature 900 °C | 182 BTU-in/hr-ft²-°F @Temperature 1650 °F |
| 28.0 W/m-K @Temperature 1000 °C | 194 BTU-in/hr-ft²-°F @Temperature 1830 °F |
| 29.5 W/m-K @Temperature 1100 °C | 205 BTU-in/hr-ft²-°F @Temperature 2010 °F |
Melting Point | 1270 - 1377 °C | 2320 - 2511 °F |
Solidus | 1270 °C | 2320 °F |
Liquidus | 1377 °C | 2511 °F |
|
Processing Properties | Metric | English | Comments |
---|
Annealing Temperature | 954 - 1066 °C | 1750 - 1951 °F |
Hot-Working Temperature | 930 - 1150 °C | 1710 - 2100 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Aluminum, Al | 0.010 - 0.70 % | 0.010 - 0.70 % |
Carbon, C | 0.0050 - 0.040 % | 0.0050 - 0.040 % |
Chromium, Cr | 19.5 - 23 % | 19.5 - 23 % |
Copper, Cu | 1.5 - 3.0 % | 1.5 - 3.0 % |
Iron, Fe | 5.7 - 28 % | 5.7 - 28 % |
Manganese, Mn | <= 1.0 % | <= 1.0 % |
Molybdenum, Mo | 3.0 - 4.0 % | 3.0 - 4.0 % |
Nickel, Ni | 45 - 55 % | 45 - 55 % |
Niobium, Nb (Columbium, Cb) | 2.5 - 4.5 % | 2.5 - 4.5 % |
Phosphorus, P | <= 0.030 % | <= 0.030 % |
Silicon, Si | <= 0.50 % | <= 0.50 % |
Sulfur, S | <= 0.030 % | <= 0.030 % |
Titanium, Ti | 0.50 - 2.5 % | 0.50 - 2.5 % |