Physical Properties | Metric | English | Comments |
---|
Density | 8.69 g/cc | 0.314 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell B | 93 @Temperature 23.0 °C | 93 @Temperature 73.4 °F |
| 95 @Temperature 23.0 °C | 95 @Temperature 73.4 °F |
Tensile Strength, Ultimate | 490 MPa @Thickness 12.7 mm, Temperature 760 °C | 71100 psi @Thickness 0.500 in, Temperature 1400 °F |
| 545 MPa @Thickness 3.17 mm, Temperature 538 °C | 79000 psi @Thickness 0.125 in, Temperature 1000 °F |
| 593 MPa @Thickness 12.7 mm, Temperature 538 °C | 86000 psi @Thickness 0.500 in, Temperature 1000 °F |
| 607 MPa @Thickness 6.35 mm, Temperature 538 °C | 88000 psi @Thickness 0.250 in, Temperature 1000 °F |
| 745 MPa @Thickness 3.17 mm, Temperature 20.0 °C | 108000 psi @Thickness 0.125 in, Temperature 68.0 °F |
| 786 MPa @Thickness 12.7 mm, Temperature 20.0 °C | 114000 psi @Thickness 0.500 in, Temperature 68.0 °F |
| 800 MPa @Thickness 6.35 mm, Temperature 20.0 °C | 116000 psi @Thickness 0.250 in, Temperature 68.0 °F |
Tensile Strength, Yield | 248 MPa @Thickness 6.35 mm, Temperature 538 °C | 36000 psi @Thickness 0.250 in, Temperature 1000 °F |
| 269 MPa @Thickness 12.7 mm, Temperature 760 °C | 39000 psi @Thickness 0.500 in, Temperature 1400 °F |
| 276 MPa @Thickness 3.17 mm, Temperature 538 °C | 40000 psi @Thickness 0.125 in, Temperature 1000 °F |
| 310 MPa @Thickness 12.7 mm, Temperature 538 °C | 45000 psi @Thickness 0.500 in, Temperature 1000 °F |
| 386 MPa @Thickness 6.35 mm, Temperature 20.0 °C | 56000 psi @Thickness 0.250 in, Temperature 68.0 °F |
| 421 MPa @Thickness 3.17 mm, Temperature 20.0 °C | 61100 psi @Thickness 0.125 in, Temperature 68.0 °F |
| 448 MPa @Thickness 12.7 mm, Temperature 20.0 °C | 65000 psi @Thickness 0.500 in, Temperature 68.0 °F |
Elongation at Break | 23 % @Thickness 3.17 mm, Temperature 538 °C | 23 % @Thickness 0.125 in, Temperature 1000 °F |
| 30 % @Thickness 3.17 mm, Temperature 20.0 °C | 30 % @Thickness 0.125 in, Temperature 68.0 °F |
| 30 % @Thickness 12.7 mm, Temperature 760 °C | 30 % @Thickness 0.500 in, Temperature 1400 °F |
| 47 % @Thickness 12.7 mm, Temperature 20.0 °C | 47 % @Thickness 0.500 in, Temperature 68.0 °F |
| 51 % @Thickness 6.35 mm, Temperature 538 °C | 51 % @Thickness 0.250 in, Temperature 1000 °F |
| 52 % @Thickness 12.7 mm, Temperature 538 °C | 52 % @Thickness 0.500 in, Temperature 1000 °F |
| 60 % @Thickness 6.35 mm, Temperature 20.0 °C | 60 % @Thickness 0.250 in, Temperature 68.0 °F |
Modulus of Elasticity | 206 GPa | 29900 ksi |
| 145 GPa @Temperature 982 °C | 21000 ksi @Temperature 1800 °F |
| 154 GPa @Temperature 871 °C | 22300 ksi @Temperature 1600 °F |
| 163 GPa @Temperature 760 °C | 23600 ksi @Temperature 1400 °F |
| 171 GPa @Temperature 649 °C | 24800 ksi @Temperature 1200 °F |
| 177 GPa @Temperature 538 °C | 25700 ksi @Temperature 1000 °F |
| 183 GPa @Temperature 427 °C | 26500 ksi @Temperature 801 °F |
| 190 GPa @Temperature 316 °C | 27600 ksi @Temperature 601 °F |
| 196 GPa @Temperature 204 °C | 28400 ksi @Temperature 399 °F |
| 203 GPa @Temperature 93.0 °C | 29400 ksi @Temperature 199 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.000114 ohm-cm @Temperature 24.0 °C | 0.000114 ohm-cm @Temperature 75.2 °F |
| 0.000123 ohm-cm @Temperature 100 °C | 0.000123 ohm-cm @Temperature 212 °F |
| 0.000124 ohm-cm @Temperature 200 °C | 0.000124 ohm-cm @Temperature 392 °F |
| 0.000125 ohm-cm @Temperature 300 °C | 0.000125 ohm-cm @Temperature 572 °F |
| 0.000126 ohm-cm @Temperature 400 °C | 0.000126 ohm-cm @Temperature 752 °F |
| 0.000127 ohm-cm @Temperature 500 °C | 0.000127 ohm-cm @Temperature 932 °F |
| 0.000128 ohm-cm @Temperature 600 °C | 0.000128 ohm-cm @Temperature 1110 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 12.4 µm/m-°C @Temperature 24.0 - 93.0 °C | 6.89 µin/in-°F @Temperature 75.2 - 199 °F |
| 12.4 µm/m-°C @Temperature 24.0 - 204 °C | 6.89 µin/in-°F @Temperature 75.2 - 399 °F |
| 12.6 µm/m-°C @Temperature 24.0 - 316 °C | 7.00 µin/in-°F @Temperature 75.2 - 601 °F |
| 13.3 µm/m-°C @Temperature 24.0 - 427 °C | 7.39 µin/in-°F @Temperature 75.2 - 801 °F |
| 13.9 µm/m-°C @Temperature 24.0 - 538 °C | 7.72 µin/in-°F @Temperature 75.2 - 1000 °F |
| 14.6 µm/m-°C @Temperature 24.0 - 649 °C | 8.11 µin/in-°F @Temperature 75.2 - 1200 °F |
| 15.3 µm/m-°C @Temperature 24.0 - 760 °C | 8.50 µin/in-°F @Temperature 75.2 - 1400 °F |
| 15.8 µm/m-°C @Temperature 24.0 - 871 °C | 8.78 µin/in-°F @Temperature 75.2 - 1600 °F |
| 16.2 µm/m-°C @Temperature 24.0 - 982 °C | 9.00 µin/in-°F @Temperature 75.2 - 1800 °F |
Specific Heat Capacity | 0.414 J/g-°C @Temperature 52.0 °C | 0.0989 BTU/lb-°F @Temperature 126 °F |
| 0.423 J/g-°C @Temperature 100 °C | 0.101 BTU/lb-°F @Temperature 212 °F |
| 0.444 J/g-°C @Temperature 200 °C | 0.106 BTU/lb-°F @Temperature 392 °F |
| 0.460 J/g-°C @Temperature 300 °C | 0.110 BTU/lb-°F @Temperature 572 °F |
| 0.476 J/g-°C @Temperature 400 °C | 0.114 BTU/lb-°F @Temperature 752 °F |
| 0.489 J/g-°C @Temperature 500 °C | 0.117 BTU/lb-°F @Temperature 932 °F |
| 0.514 J/g-°C @Temperature 600 °C | 0.123 BTU/lb-°F @Temperature 1110 °F |
Thermal Conductivity | 10.1 W/m-K @Temperature 48.0 °C | 70.1 BTU-in/hr-ft²-°F @Temperature 118 °F |
| 11.1 W/m-K @Temperature 100 °C | 77.0 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 13.4 W/m-K @Temperature 200 °C | 93.0 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 15.5 W/m-K @Temperature 300 °C | 108 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 17.5 W/m-K @Temperature 400 °C | 121 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 19.5 W/m-K @Temperature 500 °C | 135 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 21.3 W/m-K @Temperature 600 °C | 148 BTU-in/hr-ft²-°F @Temperature 1110 °F |
Melting Point | 1357 - 1399 °C | 2475 - 2550 °F |
Solidus | 1357 °C | 2475 °F |
Liquidus | 1399 °C | 2550 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | <= 0.010 % | <= 0.010 % |
Chromium, Cr | 22 % | 22 % |
Cobalt, Co | <= 2.5 % | <= 2.5 % |
Iron, Fe | 3.0 % | 3.0 % |
Manganese, Mn | <= 0.50 % | <= 0.50 % |
Molybdenum, Mo | 13 % | 13 % |
Nickel, Ni | 56 % | 56 % |
Silicon, Si | <= 0.080 % | <= 0.080 % |
Tungsten, W | 3.0 % | 3.0 % |
Vanadium, V | <= 0.35 % | <= 0.35 % |