MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

EDRO UltraChem® #15 Precipitation Hardening Stainless Mold Steel
Categories: Metal; Ferrous Metal; Stainless Steel; Precipitation Hardening Stainless

Material Notes: Ultrachem® is a chromium-nickel precipitation-hardening stainless steel, a modified PH alloy grade, which is characterized by: exceptional corrosion resistance, uniform hardness in all dimensions, excellent compressive strength, simple low temperature heat treatment with small dimensional change, good weldability, and excellent toughness.
Ultrachem® is normally supplied in a fully heat treated condition, age hardened to 38 or 42 HRC.
Ultrachem® is recommended for use in longlife molds subjected to severe working conditions, including corrosive materials and atmospheres, high stressed and indentation experienced in fast cycling molding operations. It better resists corrosion from the more highly corrosive plastics than AISI 420 stainless steels

Information provided by EDRO

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density  7.75 g/cc
@Temperature 399 °C
0.280 lb/in³
@Temperature 750 °F
Age-hardened to 42 HRC
 7.81 g/cc
@Temperature 199 °C
0.282 lb/in³
@Temperature 390 °F
Age-hardened to 42 HRC
 7.86 g/cc
@Temperature 20.0 °C
0.284 lb/in³
@Temperature 68.0 °F
Age-hardened to 42 HRC
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 38 - 4238 - 42
Tensile Strength, Ultimate 1310 MPa
@Temperature 20.0 °C
190000 psi
@Temperature 68.0 °F
Age hardened at 42 HRC
Tensile Strength, Yield 1210 MPa
@Temperature 20.0 °C
175000 psi
@Temperature 68.0 °F
Age hardened at 42 HRC
Elongation at Yield 14 %14 %in 2"
Reduction of Area 50 %50 %
Modulus of Elasticity  175 GPa
@Temperature 399 °C
25400 ksi
@Temperature 750 °F
 186 GPa
@Temperature 199 °C
27000 ksi
@Temperature 390 °F
 197 GPa
@Temperature 20.0 °C
28500 ksi
@Temperature 68.0 °F
Charpy Impact 33.9 J
@Temperature 20.0 °C
25.0 ft-lb
@Temperature 68.0 °F
Age hardened at 42 HRC
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.8 µm/m-°C
@Temperature 20.0 - 199 °C
6.00 µin/in-°F
@Temperature 68.0 - 390 °F
 11.7 µm/m-°C
@Temperature 20.0 - 399 °C
6.50 µin/in-°F
@Temperature 68.0 - 750 °F
Specific Heat Capacity 0.460 J/g-°C
@Temperature 20.0 °C
0.110 BTU/lb-°F
@Temperature 68.0 °F
Thermal Conductivity  16.1 W/m-K
@Temperature 20.0 °C
112 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 18.6 W/m-K
@Temperature 199 °C
129 BTU-in/hr-ft²-°F
@Temperature 390 °F
 21.5 W/m-K
@Temperature 399 °C
149 BTU-in/hr-ft²-°F
@Temperature 750 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.040 %0.040 %
Chromium, Cr 14.75 %14.75 %
Copper, Cu 3.2 %3.2 %
Iron, Fe 76.68 %76.68 %As Balance
Manganese, Mn 0.50 %0.50 %
Nickel, Ni 4.5 %4.5 %
Niobium, Nb (Columbium, Cb) 0.25 %0.25 %
Sulfur, S 0.080 %0.080 %
 
Descriptive Properties
Color CodeWhite

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
EDRO #7 Shock Resistant S7 Tool Steel
EDRO P1FM #31 Free Machining Holder Steel
EDRO #5 H13-Hot Work Tool Steel
EDRO EDRO400™ #40 Prehardened Insert Quality Martensitic Stainless Steel
EDRO RoyAlloy™ #6 Free Machining Stainless Holder Steel

NSEDRO005 / 142942

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.