AISI 4140H Steel, annealed 815°C
Categories:
Metal
;
Ferrous Metal
;
Alloy Steel
;
AISI 4000 Series Steel
;
Low Alloy Steel
;
Carbon Steel
;
Medium Carbon Steel
Key Words:
AFNOR 40 CD 4, AFNOR 42 CD 4, JIS SCM 4 H, JIS SCM440, SS14 2244 (Sweden), B.S. 708 A 42 (UK), B.S. 708 M 40 (UK), B.S. 709 M 40 (UK), UNS H41400, ASTM A304, SAE J1268, DIN 1.7225
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
7.85
g/cc
0.284
lb/in³
Mechanical Properties
Metric
English
Comments
Hardness, Brinell
197
197
Hardness, Knoop
219
219
Converted from Brinell
Hardness, Rockwell B
92
92
Converted from Brinell
Hardness, Rockwell C
13
13
Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
Hardness, Vickers
207
207
Converted from Brinell
Tensile Strength, Ultimate
655
MPa
95000
psi
Tensile Strength, Yield
420
MPa
60900
psi
Elongation at Break
25.7 %
25.7 %
Modulus of Elasticity
205
GPa
29700
ksi
Typical for steel
Bulk Modulus
160
GPa
23200
ksi
Typical for steel
Poissons Ratio
0.29
0.29
Calculated
Machinability
65 %
65 %
Based on AISI 1212 as 100% machinability.
Shear Modulus
80.0
GPa
11600
ksi
Typical for steel
Izod Impact
54.0
J
39.8
ft-lb
Electrical Properties
Metric
English
Comments
Electrical Resistivity
0.0000220
ohm-cm
@Temperature 20.0 °C
0.0000220
ohm-cm
@Temperature 68.0 °F
specimen hardened and tempered
0.0000263
ohm-cm
@Temperature 100 °C
0.0000263
ohm-cm
@Temperature 212 °F
specimen hardened and tempered
0.0000326
ohm-cm
@Temperature 200 °C
0.0000326
ohm-cm
@Temperature 392 °F
specimen hardened and tempered
0.0000475
ohm-cm
@Temperature 400 °C
0.0000475
ohm-cm
@Temperature 752 °F
specimen hardened and tempered
0.0000646
ohm-cm
@Temperature 600 °C
0.0000646
ohm-cm
@Temperature 1110 °F
specimen hardened and tempered
Thermal Properties
Metric
English
Comments
CTE, linear
12.2
µm/m-°C
@Temperature 0.000 - 100 °C
6.78
µin/in-°F
@Temperature 32.0 - 212 °F
13.7
µm/m-°C
@Temperature 20.0 - 400 °C
7.61
µin/in-°F
@Temperature 68.0 - 752 °F
14.6
µm/m-°C
@Temperature 20.0 - 600 °C
8.11
µin/in-°F
@Temperature 68.0 - 1110 °F
Specific Heat Capacity
0.473
J/g-°C
@Temperature 150 - 200 °C
0.113
BTU/lb-°F
@Temperature 302 - 392 °F
0.519
J/g-°C
@Temperature 350 - 400 °C
0.124
BTU/lb-°F
@Temperature 662 - 752 °F
0.561
J/g-°C
@Temperature 550 - 600 °C
0.134
BTU/lb-°F
@Temperature 1020 - 1110 °F
Thermal Conductivity
42.6
W/m-K
296
BTU-in/hr-ft²-°F
Component Elements Properties
Metric
English
Comments
Carbon, C
0.37 - 0.44 %
0.37 - 0.44 %
Chromium, Cr
0.75 - 1.2 %
0.75 - 1.2 %
Iron, Fe
96.585 - 97.93 %
96.585 - 97.93 %
As remainder
Manganese, Mn
0.65 - 1.1 %
0.65 - 1.1 %
Molybdenum, Mo
0.15 - 0.30 %
0.15 - 0.30 %
Phosphorus, P
<= 0.035 %
<= 0.035 %
Silicon, Si
0.15 - 0.30 %
0.15 - 0.30 %
Sulfur, S
<= 0.040 %
<= 0.040 %
References
for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
AISI 4140H Steel, normalized at 870°C
AISI 4140 Steel, annealed at 815°C (1500°F) furnace cooled 11°C (20°F)/hour to 665°C (1230°F), air cooled, 25 mm (1 in.) round
AISI 1018 Steel, cold drawn
AISI 4140H Steel, annealed 25 mm (1 in.) round
AISI 4140H Steel, heat treated, tempered 205°C (400°F), 25 mm (1 in.) round
M414BE / 7590
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.