MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

RTP Company ESD C 101 FR Polypropylene (PP), Glass Fiber - ESD Protection - Electrically Conductive - Flame Retardant
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 10% Glass Fiber Filler

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.42 g/cc1.42 g/ccASTM D 792
Additive Loading 10 %10 %Primary Additive
Linear Mold Shrinkage 0.0030 - 0.0050 cm/cm
@Thickness 3.20 mm
0.0030 - 0.0050 in/in
@Thickness 0.126 in
ASTM D 955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 25.5 MPa3700 psiASTM D 638
Elongation at Break 2.0 - 4.0 %2.0 - 4.0 %ASTM D 638
Tensile Modulus 3.79 GPa550 ksiASTM D 638
Flexural Strength 41.4 MPa6000 psiASTM D 790
Flexural Modulus 3.45 GPa500 ksiASTM D 790
Izod Impact, Notched 0.427 J/cm
@Thickness 3.20 mm
0.800 ft-lb/in
@Thickness 0.126 in
ASTM D 256
Izod Impact, Unnotched 1.33 J/cm
@Thickness 3.20 mm
2.50 ft-lb/in
@Thickness 0.126 in
ASTM D 4812
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity <= 1000 ohm-cm<= 1000 ohm-cmASTM D 257
Surface Resistance <= 1e+05<= 1e+05ESD STM11.11
Surface Resistivity per Square <= 1.00e+6 ohm<= 1.00e+6 ohmASTM D 257; ESD STM11.11
Static Decay <= 2.0 sec<= 2.0 secMIL-PRF-81705D, 5kV to 50 V, 12% RH; FTMS101C; 4046.1
 
Thermal PropertiesMetricEnglishComments
Flammability, UL94 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature 191 - 232 °C375 - 450 °F
Mold Temperature 32.2 - 65.6 °C90.0 - 150 °F
Drying Temperature 79.4 °C
@Time 7200 sec
175 °F
@Time 2.00 hour
Injection Pressure 68.9 - 103 MPa10000 - 15000 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
RTP Company RTP 154 Polypropylene (PP), Flame Retardant - UL94 V-0
RTP Company RTP 100 FR Polypropylene (PP), Flame Retardant - Non-PBDE/PBB - UL94 V-0
RTP Company RTP 100 FR LF Polypropylene (PP), Low Flow - Flame Retardant - UL94 V-0
RTP Company RTP 100 FR HF Polypropylene (PP), High Flow - Flame Retardant - UL94 V-0
RTP Company RTP 105 CC FR Polypropylene (PP), Glass Fiber - Chemically Coupled - Flame Retardant - UL94 V-0

PQZWA7575 / 92308

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.