MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Polyram RamSter PF305G6 PBT, 30% Glass Fiber
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled

Material Notes: 30% Glass fiber reinforced, PBT for injection molding applications.

Information provided by Polyram.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.50 g/cc0.0542 lb/in³ISO 1183
Moisture Absorption at Equilibrium 0.10 %0.10 %50% RH; ISO 62
Water Absorption at Saturation 0.50 %0.50 %ISO 62
Linear Mold Shrinkage 0.0030 cm/cm0.0030 in/inISO 2577
Melt Flow 15 g/10 min
@Load 2.16 kg,
Temperature 250 °C
15 g/10 min
@Load 4.76 lb,
Temperature 482 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 130 MPa18900 psiISO 527
Elongation at Break 3.0 %3.0 %ISO 527
Tensile Modulus 8.10 GPa1170 ksiISO 527
Flexural Strength 180 MPa26100 psiISO 178
Flexural Modulus 8.60 GPa1250 ksiISO 178
Izod Impact, Notched (ISO)  8.50 kJ/m²
@Temperature -30.0 °C
4.04 ft-lb/in²
@Temperature -22.0 °F
ISO 180
 12.0 kJ/m²
@Temperature 23.0 °C
5.71 ft-lb/in²
@Temperature 73.4 °F
ISO 180
Charpy Impact Unnotched  7.00 J/cm²
@Temperature 23.0 °C
33.3 ft-lb/in²
@Temperature 73.4 °F
ISO 179
 7.50 J/cm²
@Temperature -30.0 °C
35.7 ft-lb/in²
@Temperature -22.0 °F
ISO 179
Charpy Impact, Notched  0.850 J/cm²
@Temperature -30.0 °C
4.04 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 1.15 J/cm²
@Temperature 23.0 °C
5.47 ft-lb/in²
@Temperature 73.4 °F
ISO 179
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmIEC 60093
Dielectric Constant 3.83.8IEC 60250
 
Thermal PropertiesMetricEnglishComments
Melting Point 225 °C437 °FISO 11357
Maximum Service Temperature, Air 130 °C266 °FContinuous use
 200 °C392 °FShort peaks operation
Deflection Temperature at 0.46 MPa (66 psi) 219 °C426 °FISO 75
Deflection Temperature at 1.8 MPa (264 psi) 206 °C403 °FISO 75
Flammability, UL94 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
Flame Spread 15 mm/min0.59 in/minFMVSS302

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Shinkong Synthetic Fibers Shinite® D201G30 PBT, 30% Glass Filled
Mitsubishi Novaduran® 5010G30 Polybutylene Terephthalate
Celanese Nilit Nilitop BT G6 General Purpose, 30% Glass Fiber Reinforced PBT
LG Chemical Lupox® GP2300R PBT+GF30%
Polyplastics Duranex® 3300 Polybutylene Terephthalate (PBT), Standard, 30% GF filled

PPOLYR913 / 126710

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.