MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Kolon SPESIN® KP213G30 Flame Retardant PBT Resin
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Flame Retardant

Material Notes: SPESIN® is a thermoplastic PBT resin with excellent thermal, mechanical and electrical properties. SPESIN® is widely used in industrial parts and especially in electrical-electronic parts.

High heat stability, outstanding abrasion resistance, excellent electrical properties, good surface gloss, low water absorption, excellent chemical resistance, good processability

Information provided by US distributor, API-Kolon.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.52 g/cc0.0549 lb/in³DIN 53479; ASTM D792
Water Absorption 0.050 %0.050 %DIN 53475; ASTM D570
Linear Mold Shrinkage 0.0050 - 0.010 cm/cm0.0050 - 0.010 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 119119DIN 53505; ASTM D785
Tensile Strength, Ultimate 137 MPa19900 psiDIN 53455; ASTM D638
Elongation at Break 5.0 %5.0 %DIN 53455; ASTM D638
Flexural Yield Strength 211 MPa30600 psiDIN 53455; ASTM D790
Flexural Modulus 8.34 GPa1210 ksiDIN 53452; ASTM D790
Izod Impact, Notched 0.883 J/cm1.65 ft-lb/inDIN 53453; ASTM D256
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant 3.2
@Frequency 1e+6 Hz
3.2
@Frequency 1e+6 Hz
ASTM D150/DIN 53483
Dielectric Strength 30.0 kV/mm762 kV/inASTM D149/DIN 53481
Arc Resistance 120 sec120 secASTM D495
 
Thermal PropertiesMetricEnglishComments
CTE, linear 40.0 µm/m-°C
@Temperature 20.0 °C
22.2 µin/in-°F
@Temperature 68.0 °F
DIN 53752; ASTM D696
Melting Point 224 °C435 °FDIN 53736; ASTM D789
Deflection Temperature at 0.46 MPa (66 psi) 220 °C428 °FDIN 53461; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 205 °C401 °FDIN 53461; ASTM D648
Flammability, UL94 HBHB

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Capron® 8233G 33% Glass-Filled Nylon 6 (Dry)
Tipco Tipcolene® CR 8233 - 20% Talc/Mineral Reinforced Polypropylene Copolymer Compound
Polyplastics Duranex® 6300T Polybutylene Terephthalate (PBT), Low friction, Low wear, Mineral filled
Overview of materials for Polybutylene Terephthalate (PBT), Flame Retardant
Kolon SPESIN® KP212VO Flame Retardant PBT Resin

PKOL065 / 48971

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.