MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI Type 430Ti Stainless Steel annealed 1.6 mm thickness
Categories: Metal; Ferrous Metal; Stainless Steel; T 400 Series Stainless Steel

Material Notes: Titanium minimum of 6 times Carbon content

Key Words: UNS S43036, ASTM A268, ASTM A554, ASTM A651, DIN 1.4510
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 78 - 8678 - 86
Tensile Strength, Ultimate 483 MPa70100 psi
Tensile Strength, Yield 328 MPa47600 psi
Elongation at Break 30 %30 %in 50 mm
Modulus of Elasticity 200 GPa29000 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000610 ohm-cm0.0000610 ohm-cm
Magnetic Permeability 600 - 1100600 - 1100annealed condition at RT
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.1 µm/m-°C
@Temperature 20.0 - 100 °C
5.61 µin/in-°F
@Temperature 68.0 - 212 °F
 11.5 µm/m-°C
@Temperature 20.0 - 500 °C
6.39 µin/in-°F
@Temperature 68.0 - 932 °F
 12.4 µm/m-°C
@Temperature 20.0 - 800 °C
6.89 µin/in-°F
@Temperature 68.0 - 1470 °F
Specific Heat Capacity 0.460 J/g-°C
@Temperature 0.000 - 100 °C
0.110 BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity 24.2 W/m-K
@Temperature 0.000 - 100 °C
168 BTU-in/hr-ft²-°F
@Temperature 32.0 - 212 °F
Maximum Service Temperature, Air 815 °C1500 °FContinuous Service
 870 °C1600 °FIntermittent
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.070 %<= 0.070 %
Chromium, Cr 18 %18 %
Iron, Fe 79 %79 %
Manganese, Mn <= 1.0 %<= 1.0 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %
Titanium, Ti <= 1.1 %<= 1.1 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type 430F(Se) Stainless Steel
430 Stainless Steel annealed sheet
AISI Type 430F Stainless Steel
430 Stainless Steel annealed plate
AISI Type 430F Stainless Steel annealed bar

MQ430VA / 13150

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.