MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

EMS-Grivory Grivory® GV-6H EF black 9915 PA*-GF60
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA)

Material Notes: Product description: Grivory GV-6H black 9915 is a 60% glass fiber reinforced engineering thermoplastic material based on a combination of semicrystalline Polyamide with partially aromatic copolyamide. Grivory GV-6H black 9915 is used for injection molding technical parts, exhibiting exceptional characteristics even after moisture absorption:
  • high stiffness and strength
  • dimensional stability, low warpage
  • good chemical resistance
  • good surface finish
Grivory GV is the economical alternative to die-cast alloys.

Information provided by EMS Grivory

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.69 g/cc0.0611 lb/in³Dry; ISO 1183
Water Absorption 3.5 %3.5 %Sim. to ISO 62
Moisture Absorption 1.20 %1.20 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0010 cm/cm0.0010 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0030 cm/cm0.0030 in/inISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 290 MPa42100 psiConditioned; ISO 2039-1
 315 MPa45700 psiDry; ISO 2039-1
Tensile Strength at Break 240 MPa34800 psiConditioned; ISO 527-1/-2
 260 MPa37700 psiDry; ISO 527-1/-2
Elongation at Break 2.0 %2.0 %Dry; ISO 527-1/-2
 2.0 %2.0 %Conditioned; ISO 527-1/-2
Tensile Modulus 21.0 GPa3050 ksiConditioned; ISO 527-1/-2
 22.0 GPa3190 ksiDry; ISO 527-1/-2
Charpy Impact Unnotched  8.00 J/cm²
@Temperature 23.0 °C
38.1 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eU
 8.00 J/cm²
@Temperature -30.0 °C
38.1 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eU
 8.00 J/cm²
@Temperature 23.0 °C
38.1 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eU
 8.00 J/cm²
@Temperature -30.0 °C
38.1 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eU
Charpy Impact, Notched  1.30 J/cm²
@Temperature -30.0 °C
6.19 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eA
 1.30 J/cm²
@Temperature -30.0 °C
6.19 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eA
 1.40 J/cm²
@Temperature 23.0 °C
6.66 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eA
 1.40 J/cm²
@Temperature 23.0 °C
6.66 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+10 ohm-cm1.00e+10 ohm-cmConditioned; IEC 60093
 1.00e+12 ohm-cm1.00e+12 ohm-cmDry; IEC 60093
Surface Resistance 1.00e+11 ohm1.00e+11 ohmIEC 60093
Dielectric Strength 33.0 kV/mm838 kV/inDry; IEC 60243-1
 33.0 kV/mm838 kV/inConditioned; IEC 60243-1
Comparative Tracking Index 600 V600 VConditioned; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 15.0 µm/m-°C8.33 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 90.0 µm/m-°C50.0 µin/in-°FISO 11359-1/-2
Melting Point 260 °C500 °F10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 100 - 120 °C212 - 248 °FLong Term; ISO 2578
 220 °C428 °FShort Term; EMS
Deflection Temperature at 1.8 MPa (264 psi) 235 °C455 °FISO 75-1/-2
Deflection Temperature at 8.0 MPa 175 °C347 °FISO 75-1/-2
Flammability, UL94 HBHBIEC 60695-11-10
 
Descriptive Properties
AutomotiveAir intake systems
 Compressed air systems
 Cooling and climate control
 Exterior
 Fuel systems
Electricals & ElectronicsConnectors
 Electrical appliances
 Electrical equipment
 Energy distribution
 Lighting
 Mobile phones and other portable devices
FormGranules
ProcessingInjection Molding
Product AttributesBarrier Properties
 Co Polyamide
 High viscosity
 Long Fiber Reinforced
 Masterbatch
 Nucleated
 Transparent Polyamide

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 66, 60% Glass Fiber Filled
EMS-Grivory Grilon® BG-60 FC PA6-GF60
Evonik Trogamid® CX7323 Transparent Nylon
EMS-Grivory Grilon® AG-30 H PA66
EMS-Grivory Grivory® HTV-3H1 black 9205 PA6T/6I-GF30

PGRH341 / 157050

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.