MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

SEKISUI SPI KYDEX® 6565 Thermoplastic
Categories: Polymer; Thermoplastic

Material Notes: Low heat release aviation sheet

KYDEX® 6565 is a proprietary, high performance thermoplastic sheet specifically formulated to meet the safety needs of the aviation industry

KYDEX® 6565 meets all fire retardancy requirements set forth in Federal Aviation Regulations 25.853 paragraphs (a) and (d) (old (c)) including low heat release (65/65) in the OSU rate of heat release test. Its excellent properties make it the ideal material to form two and three-dimensional aircraft components.

Suggested Applications:

  • Seat parts
  • Window shades
  • Life vest shrouds
  • Passenger service units
  • Monitor shrouds
  • Bulkhead laminates
  • Armrests
  • Molding strips
  • Tray tables
  • Kick panels

Features:

  • Available in over 200 developed colors, various textures and thicknesses from 0.71 mm (0.028 in) and up
  • Easy to clean with aggressive cleaners and citrus-based cleaners (avoid ammoniated cleaners)
  • Meets the stringent requirements of FAR 25.853 paragraph (d) in all thicknesses and colors
  • Forms deep draws with low forces when heated to the upper end of forming temperature range
  • Crisp detail, minimal rejects
  • Can be formed on all standard presses and cut on all standard die-cutting machines
  • Secondary operations include: machining, sawing, blanking, punching, etc., are easily performed

Values based upon 3.18 mm (0.125 in) sheet unless otherwise specified

Information provided by Sekisui Polymer Innovations

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.48 g/cc1.48 g/ccASTM D792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 9898ASTM D785
Tensile Strength 45.0 MPa6530 psiASTM D638
Modulus of Elasticity 2.896 GPa420.0 ksiASTM D790
Flexural Strength 70.0 MPa10200 psiASTM D790
Impact Test  7.24 J
@Temperature 22.8 °C
5.34 ft-lb
@Temperature 73.0 °F
Dynatup; Max. Energy
 131 J
@Temperature 22.8 °C
96.7 ft-lb
@Temperature 73.0 °F
Dynatup; Cum. Energy
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 78.3 °C173 °FAnnealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Processing Temperature 163 - 199 °C325 - 390 °FForming Temperature
 
Descriptive Properties
Flammability<65 kW/m²FAR 25.853(d) Part IV; OSU Heat Release
 <65 kW-min/m²FAR 25.853(d) Part IV; OSU Heat Release
 Dmax<200FAR 25.853(d) Part V; NBS Smoke Density
 PassFAR 25.853(a)(i); Vertical Burn, 60 sec
 PassFAR 25.853(a)(ii); Vertical Burn, 12 sec

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 2024-T3
Stratasys® Ultem 9085 for Rapid Prototyping
Breplast Bretene SPF Thermoplastic Composite, 40% PP + 60% PE
Breplast Bretene SPF M Thermoplastic Composite, 70% PP + 30% PE
SEKISUI SPI KYDEX® T Thermoplastic

PSEKIS044 / 185869

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.