MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

J6 Polymers JFOAM™ BX-190 Engineered Specialty Foam
Categories: Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane Foam, Unreinforced

Material Notes: JFOAM™ BX-190-R is the resin component of a two part polyurethane system, which when combined with the T component, Isocyanate, will produce a water-blown rigid polyurethane foam system. BX-190 issued for void fill and core material applications and can meet some military specifications.

Information provided by J6 Polymers LLC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.0314 g/cc0.00113 lb/in³Cup density, #10
 0.0384 g/cc0.00139 lb/in³Core; ASTM D1622
 1.07 g/cc0.0387 lb/in³R Component, Polyol Blend
 1.24 g/cc0.0448 lb/in³T Component, Polymeric MDI
Water Absorption 11.63 %11.63 %ASTM D2842
Viscosity 200 cP200 cPT Component, Polymeric MDI
 1500 cP1500 cPR Component, Polyol Blend
Storage Temperature 18.3 - 29.4 °C65.0 - 85.0 °F
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 3.25 MPa472 psiParallel; ASTM D1623
 21.26 MPa3083 psiModulus; ASTM D1623
Tensile Modulus  0.000288 GPa
@Temperature 71.1 °C
0.0417 ksi
@Temperature 160 °F
Parallel; ASTM D1623
 0.01459 GPa
@Temperature 71.1 °C
2.116 ksi
@Temperature 160 °F
Modulus; ASTM D1623
Compressive Strength  0.170 MPa
@Temperature 71.1 °C
24.6 psi
@Temperature 160 °F
Parallel, 10% deflection; ASTM D1621
 0.307 MPa
@Temperature 25.0 °C
44.5 psi
@Temperature 77.0 °F
Parallel, 10% deflection; ASTM D1621
 4.02 MPa
@Temperature 71.1 °C
583 psi
@Temperature 160 °F
Modulus, 10% deflection; ASTM D1621
 6.62 MPa
@Temperature 25.0 °C
960 psi
@Temperature 77.0 °F
Modulus, 10% deflection; ASTM D1621
Shear Modulus 0.007074 GPa1.026 ksiASTM C723
Shear Strength 0.169 MPa24.5 psiASTM C723
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity 0.0245 W/m-K0.170 BTU-in/hr-ft²-°FK-Factor; ASTM C518
 
Processing PropertiesMetricEnglishComments
Shelf Life 6.00 Month6.00 Month
 
Descriptive Properties
Dimensional Stability+0.8% Change1 day, 70°C at 100% RH, ASTM D2126
 -0.16% Change1 day, -29°C, ASTM D2126
 -0.96% Change7 days, -29°C, ASTM D2126
 -1.32% Change14 days, 93.3°C, ASTM D2126
 -1.39% Change7 days, 93.3°C, ASTM D2126
 -1.39% Change7 days, 70°C at 100% RH, ASTM D2126
 -1.45% Change1 day, 93.3°C, ASTM D2126
 -1.53% Change14 days, 70°C at 100% RH, ASTM D2126
 -1.56% Change14 days, -29°C, ASTM D2126
Friability0.1337ASTM C421
Hand Mix Reactivity21 secCream Time
Mixing Ratio0.3R Component, Polyol Blend
 0.7T Component, Polymeric MDI

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
J6 Polymers JFOAM™ A-204 Engineered Specialty Foam
3M RPF-C (0.32 g/cc) (Reinforced Polyurethane Foam) Continuous Strand Fiberglass
3M RPF-C (0.24 g/cc) (Reinforced Polyurethane Foam) Continuous Strand Fiberglass
General Plastics LAST-A-FOAM® R-9320 Thermal Isolation Blocks
General Plastics LAST-A-FOAM® TR-20 Polyurethane Foam

PJSIX007 / 190934

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.