MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Okulen® 500 PE-HMW, Natural
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE)

Material Notes: OKULEN® 500 is a high molecular low pressure polyethylene with a molecular weight of approximately 500 g/mol. Applications include the food industyr and sports center construction. It does an excellent job with its impact strength and insulating properties.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.950 g/cc0.0343 lb/in³ISO 1183-A
Water Absorption <= 0.10 %<= 0.10 %
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 65
@Thickness 5.00 mm
65
@Thickness 0.197 in
3 s value; plate; ISO 868
Tensile Strength, Yield 26.0 MPa3770 psi50 mm/min; ISO/R 527
Elongation at Break >= 50 %>= 50 %50 mm/min; ISO/R 527
Creep Strength 10.0 MPa
@Temperature 20.0 °C,
Time 605000 sec
1450 psi
@Temperature 68.0 °F,
Time 168 hour
Charpy Impact Unnotched 2.50 J/cm²11.9 ft-lb/in²ISO 11542-2
Coefficient of Friction, Dynamic 0.20
@Pressure 2.00 MPa
0.20
@Pressure 290 psi
PE-metal, V = 10 m/min; ASTM D1894
Abrasion 400400Slurry-Test rel to GUR 4120 = 100%; DIN 58836
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+14 ohm-cm>= 1.00e+14 ohm-cmTeil 30; IEC 600093 / VDE 0303
Surface Resistance >= 1.00e+13 ohm>= 1.00e+13 ohmTeil 30; IEC 60093 / VDE 0303
 
Thermal PropertiesMetricEnglishComments
CTE, linear 200 µm/m-°C111 µin/in-°FDIN 53752
Melting Point 130 - 135 °C266 - 275 °FDSC ISO 3146
Maximum Service Temperature, Air 80.0 °C176 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Orbilan ORBILAN® PE 500 HMW-PE
Okulen® 500 PE-HMW, AST
Okulen® 500 PE-HMW, UV - stabilized
Okulen® 500 PE-HMW, Coloured
Nylacast PA6C Cast Nylon 6

POKUL001 / 83443

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.