MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Special Metals NI-SPAN-C® Alloy 902
Categories: Metal; Superalloy; Iron Base

Material Notes: A nickel-iron-chromium alloy made precipitation hardenable by additions of aluminum and titanium. The titanium content also helps provide a controllable thermoelastic coefficient, which is the alloy's outstanding characteristic. The alloy can be processed to have a constant modulus of elasticity at temperatures from -50°F to 150°F (-45 to 65°C). Used for precision springs, mechanical resonators, and other precision elastic components. Standard product forms are round, strip, tube, pipe, and wire.

Data provided by the manufacturer, Special Metals.

Key Words: Ni SPAN C 902, Nispan C, UNS N09902; BS 3127; SAE AMS 5210, 5221, 5223, 5225
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.05 g/cc0.291 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 1210 MPa175000 psiPrecipitation Hardened
Tensile Strength, Yield 760 MPa
@Strain 0.2 %
110000 psi
@Strain 0.2 %
Precipitation Hardened
Elongation at Break 25 %25 %Precipitation Hardened
Modulus of Elasticity 165 - 200 GPa23900 - 29000 ksi
Shear Modulus 62.0 - 69.0 GPa8990 - 10000 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000102 ohm-cm0.000102 ohm-cm
Curie Temperature 190 °C374 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear 7.60 µm/m-°C
@Temperature 20.0 - 100 °C
4.22 µin/in-°F
@Temperature 68.0 - 212 °F
Specific Heat Capacity 0.500 J/g-°C0.120 BTU/lb-°F
Thermal Conductivity 12.1 W/m-K84.0 BTU-in/hr-ft²-°F
Melting Point 1450 - 1480 °C2640 - 2700 °F
Solidus 1450 °C2640 °F
Liquidus 1480 °C2700 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 0.30 - 0.80 %0.30 - 0.80 %
Carbon, C <= 0.060 %<= 0.060 %
Chromium, Cr 4.9 - 5.75 %4.9 - 5.75 %
Iron, Fe 47 %47 %As remainder
Manganese, Mn <= 0.80 %<= 0.80 %
Nickel, Ni 41 - 43.5 %41 - 43.5 %Including Cobalt
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.040 %<= 0.040 %
Titanium, Ti 2.2 - 2.75 %2.2 - 2.75 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
California Fine Wire Alloy 52 Nickel Iron Alloy
Special Metals INCOLOY® Alloy 903
Special Metals INCOLOY® Alloy 907
Special Metals INCOLOY® Alloy 909
304 Stainless Steel

NINC83 / 17426

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.