MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

EMS-Grivory Grilamid® LKN-5H PA12-GB50
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12); Nylon 12, Glass Bead Filled

Material Notes: Product description: Grilamid LKN-5H is a 50% glass bead reinforced, heat stabilized polyamide 12 injection molding grade with the following property profile:
  • Very low moisture absorption
  • Extremely good tolerances can be achieved
  • Very dimensionally stable
  • Low shrinkage
  • Good sliding properties
  • High abrasion resistance
Grilamid LKN-5H is suitable for production of technical parts in the application fields of:
  • Electro
  • Electronics
  • Automotive
  • Safety technology
  • Mechanical engineering
  • Domestic appliances

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.44 g/cc0.0520 lb/in³Dry; ISO 1183
Water Absorption 0.80 %0.80 %Sim. to ISO 62
Moisture Absorption 0.400 %0.400 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0080 cm/cm0.0080 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0090 cm/cm0.0090 in/inISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 75
@Time 15.0 sec
75
@Time 0.00417 hour
Conditioned; ISO 868
Tensile Strength at Break 40.0 MPa5800 psiConditioned; ISO 527-1/-2
 50.0 MPa7250 psiDry; ISO 527-1/-2
Tensile Strength, Yield 45.0 MPa6530 psiConditioned; ISO 527-1/-2
 50.0 MPa7250 psiDry; ISO 527-1/-2
Elongation at Break 20 %20 %Nominal, Dry; ISO 527-1/-2
 25 %25 %Nominal, Conditioned; ISO 527-1/-2
Elongation at Yield 5.0 %5.0 %Dry; ISO 527-1/-2
 7.0 %7.0 %Conditioned; ISO 527-1/-2
Tensile Modulus 2.30 GPa334 ksiConditioned; ISO 527-1/-2
 2.60 GPa377 ksiDry; ISO 527-1/-2
Charpy Impact Unnotched  6.50 J/cm²
@Temperature -30.0 °C
30.9 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eU
 11.0 J/cm²
@Temperature 23.0 °C
52.3 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eU
 13.0 J/cm²
@Temperature 23.0 °C
61.9 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eU
Charpy Impact, Notched  0.400 J/cm²
@Temperature -30.0 °C
1.90 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eA
 0.400 J/cm²
@Temperature -30.0 °C
1.90 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eA
 0.500 J/cm²
@Temperature 23.0 °C
2.38 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eA
 0.500 J/cm²
@Temperature 23.0 °C
2.38 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+11 ohm-cm1.00e+11 ohm-cmConditioned; IEC 60093
Surface Resistance 1.00e+11 ohm1.00e+11 ohmIEC 60093
Dielectric Strength 35.0 kV/mm889 kV/inConditioned; IEC 60243-1
Comparative Tracking Index 600 V600 VConditioned; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 90.0 µm/m-°C50.0 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 90.0 µm/m-°C50.0 µin/in-°FISO 11359-1/-2
Melting Point 178 °C352 °F10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 90.0 - 120 °C194 - 248 °FLong Term; ISO 2578
 150 °C302 °FShort Term; EMS
Deflection Temperature at 1.8 MPa (264 psi) 65.0 °C149 °FISO 75-1/-2
Deflection Temperature at 8.0 MPa 40.0 °C104 °FISO 75-1/-2
Flammability, UL94 HBHBIEC 60695-11-10
 
Descriptive Properties
AutomotiveAutomotive electr. and electronics, lighting
 Powertrain and Chassis
Electricals & ElectronicsConnectors
 Electrical appliances
 Electrical equipment
 Mobile phones and other portable devices
FormGranules
Industry & Consumer goodsHousewares
 Mechanical Engineering
 Medical devices
 Sanitary, water and gas supply
 Tools & Accessories
ProcessingInjection Molding
Special CharacteristicsImproved UV resistance (outdoor use)
Water ContactACS
 DVGW W270
 WRAS

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
EMS-Grivory Grivory® HT3Z LF black 9564 PA*
EMS-Grivory Grilamid® LV-3H PA12-GF30
EMS-Grivory Grilon® BK-50 PA6-GB50
Techmer ES HiFill® PP GB50 50% Glass Beads Filled
EMS-Griltech Grilon® M 369 White Nylon 6 Fiber (Small Count)

PGRH069 / 156778

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.