MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Aluminum 2124-T851 (Extended High Temperature Data)
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
A Zr + Ti limit of 0.20 percent maximum may be used with this alloy designation for extruded and forged products only, but only when the supplier or producer and the purchaser have mutually so agreed. Agreement may be indicated, for example, by reference to a standard, by letter, by order note, or other means which allow the Zr + Ti limit.
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium 2124-T851; UNS A92124; QQ-A-250/29; ASTM B209; AMS 4101; AA2124-T851
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.78 g/cc0.100 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 128128500 kg load with 10 mm ball
Hardness, Knoop 161161Converted from Brinell Hardness Value
Hardness, Rockwell A 48.948.9Converted from Brinell Hardness Value
Hardness, Rockwell B 7979Converted from Brinell Hardness Value
Hardness, Vickers 146146Converted from Brinell Hardness Value
Tensile Strength, Ultimate 483 MPa70000 psiAA; Typical
 465 MPa
@Thickness 50.8 - 76.2 mm
67400 psi
@Thickness 2.00 - 3.00 in
Short transverse
 470 MPa
@Thickness 38.1 - 50.8 mm
68200 psi
@Thickness 1.50 - 2.00 in
Short transverse
 470 MPa
@Thickness 50.8 - 76.2 mm
68200 psi
@Thickness 2.00 - 3.00 in
Long transverse
 480 MPa
@Thickness 50.8 - 76.2 mm
69600 psi
@Thickness 2.00 - 3.00 in
Longitudinal
 490 MPa
@Thickness 38.1 - 50.8 mm
71100 psi
@Thickness 1.50 - 2.00 in
Longitudinal
 490 MPa
@Thickness 38.1 - 50.8 mm
71100 psi
@Thickness 1.50 - 2.00 in
Long transverse
 2.00 MPa
@Thickness 70.0 mm,
Temperature 535 °C
290 psi
@Thickness 2.76 in,
Temperature 995 °F
 16.0 MPa
@Thickness 70.0 mm,
Temperature 480 °C
2320 psi
@Thickness 2.76 in,
Temperature 896 °F
 485 MPa
@Thickness 70.0 mm,
Temperature 24.0 °C
70300 psi
@Thickness 2.76 in,
Temperature 75.2 °F
 505 MPa
@Thickness 70.0 mm,
Temperature -28.0 °C
73200 psi
@Thickness 2.76 in,
Temperature -18.4 °F
 525 MPa
@Thickness 70.0 mm,
Temperature -80.0 °C
76100 psi
@Thickness 2.76 in,
Temperature -112 °F
 595 MPa
@Thickness 70.0 mm,
Temperature -195 °C
86300 psi
@Thickness 2.76 in,
Temperature -319 °F
 705 MPa
@Thickness 70.0 mm,
Temperature -269 °C
102000 psi
@Thickness 2.76 in,
Temperature -452 °F
 30.0 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 425 °C
4350 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 797 °F
 34.0 MPa
@Thickness 70.0 mm,
Temperature 370 °C,
Time 3.60e+7 sec
4930 psi
@Thickness 2.76 in,
Temperature 698 °F,
Time 10000 hour
 34.0 MPa
@Thickness 70.0 mm,
Temperature 370 °C,
Time 3.60e+8 sec
4930 psi
@Thickness 2.76 in,
Temperature 698 °F,
Time 100000 hour
 34.0 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 425 °C
4930 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 797 °F
 38.0 MPa
@Thickness 70.0 mm,
Temperature 370 °C,
Time 3.60e+6 sec
5510 psi
@Thickness 2.76 in,
Temperature 698 °F,
Time 1000 hour
 41.0 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 370 °C
5950 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 698 °F
 45.0 MPa
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+8 sec
6530 psi
@Thickness 2.76 in,
Temperature 599 °F,
Time 100000 hour
 48.0 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 370 °C
6960 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 698 °F
 52.0 MPa
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+7 sec
7540 psi
@Thickness 2.76 in,
Temperature 599 °F,
Time 10000 hour
 59.0 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 370 °C
8560 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 698 °F
 62.0 MPa
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+8 sec
8990 psi
@Thickness 2.76 in,
Temperature 500 °F,
Time 100000 hour
 62.0 MPa
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+6 sec
8990 psi
@Thickness 2.76 in,
Temperature 599 °F,
Time 1000 hour
 69.0 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 315 °C
10000 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 599 °F
 76.0 MPa
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+7 sec
11000 psi
@Thickness 2.76 in,
Temperature 500 °F,
Time 10000 hour
 76.0 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 370 °C
11000 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 698 °F
 83.0 MPa
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+8 sec
12000 psi
@Thickness 2.76 in,
Temperature 446 °F,
Time 100000 hour
 83.0 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 315 °C
12000 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 599 °F
 105 MPa
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+6 sec
15200 psi
@Thickness 2.76 in,
Temperature 500 °F,
Time 1000 hour
 110 MPa
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+7 sec
16000 psi
@Thickness 2.76 in,
Temperature 446 °F,
Time 10000 hour
 125 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+8 sec
18100 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 100000 hour
 140 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 315 °C
20300 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 599 °F
 150 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 260 °C
21800 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 500 °F
 160 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 315 °C
23200 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 599 °F
 170 MPa
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+6 sec
24700 psi
@Thickness 2.76 in,
Temperature 446 °F,
Time 1000 hour
 185 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+7 sec
26800 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 10000 hour
 205 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 260 °C
29700 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 500 °F
 220 MPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+8 sec
31900 psi
@Thickness 2.76 in,
Temperature 347 °F,
Time 100000 hour
 235 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 230 °C
34100 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 446 °F
 255 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 260 °C
37000 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 500 °F
 260 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+6 sec
37700 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 1000 hour
 270 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 260 °C
39200 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 500 °F
 275 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 230 °C
39900 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 446 °F
 295 MPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+7 sec
42800 psi
@Thickness 2.76 in,
Temperature 347 °F,
Time 10000 hour
 305 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 205 °C
44200 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 401 °F
 310 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 230 °C
45000 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 446 °F
 325 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 230 °C
47100 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 446 °F
 330 MPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+6 sec
47900 psi
@Thickness 2.76 in,
Temperature 347 °F,
Time 1000 hour
 330 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 205 °C
47900 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 401 °F
 345 MPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+8 sec
50000 psi
@Thickness 2.76 in,
Temperature 302 °F,
Time 100000 hour
 360 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 175 °C
52200 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 347 °F
 360 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 205 °C
52200 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 401 °F
 365 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 205 °C
52900 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 401 °F
 370 MPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+7 sec
53700 psi
@Thickness 2.76 in,
Temperature 302 °F,
Time 10000 hour
 380 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 175 °C
55100 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 347 °F
 385 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 175 °C
55800 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 347 °F
 397 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 175 °C
57600 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 347 °F
 400 MPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+6 sec
58000 psi
@Thickness 2.76 in,
Temperature 302 °F,
Time 1000 hour
 405 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 150 °C
58700 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 302 °F
 415 MPa
@Time 360 - 36000 sec,
Thickness 70.0 mm,
Temperature 150 °C
60200 psi
@Time 0.100 - 10.0 hour,
Thickness 2.76 in,
Temperature 302 °F
 450 MPa
@Thickness 70.0 mm,
Temperature 100 °C,
Time 3.60e+8 sec
65300 psi
@Thickness 2.76 in,
Temperature 212 °F,
Time 100000 hour
 455 MPa
@Time 360 - 3.60e+7 sec,
Thickness 70.0 mm,
Temperature 100 °C
66000 psi
@Time 0.100 - 10000 hour,
Thickness 2.76 in,
Temperature 212 °F
 485 MPa
@Treatment Temp. 24.0 °C,
Thickness 70.0 mm
70300 psi
@Treatment Temp. 75.2 °F,
Thickness 2.76 in
 185 MPa
@Time 3.60e+7 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
26800 psi
@Time 10000 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 185 MPa
@Time 3.60e+7 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
26800 psi
@Time 10000 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 195 MPa
@Time 3.60e+7 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
28300 psi
@Time 10000 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 205 MPa
@Time 3.60e+6 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
29700 psi
@Time 1000 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 215 MPa
@Time 3.60e+7 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
31200 psi
@Time 10000 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 215 MPa
@Time 3.60e+6 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
31200 psi
@Time 1000 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 235 MPa
@Time 3.60e+6 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
34100 psi
@Time 1000 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 235 MPa
@Time 360000 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
34100 psi
@Time 100 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 240 MPa
@Time 360000 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
34800 psi
@Time 100 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 255 MPa
@Time 36000 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
37000 psi
@Time 10.0 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 270 MPa
@Time 36000 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
39200 psi
@Time 10.0 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 275 MPa
@Time 1800 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
39900 psi
@Time 0.500 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 290 MPa
@Time 3.60e+7 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
42100 psi
@Time 10000 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 290 MPa
@Time 3.60e+6 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
42100 psi
@Time 1000 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 290 MPa
@Time 360000 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
42100 psi
@Time 100 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 340 MPa
@Time 1800 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
49300 psi
@Time 0.500 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 370 MPa
@Time 360000 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
53700 psi
@Time 100 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 385 MPa
@Time 36000 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
55800 psi
@Time 10.0 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 395 MPa
@Time 3.60e+6 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
57300 psi
@Time 1000 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 405 MPa
@Time 3.60e+7 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
58700 psi
@Time 10000 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 425 MPa
@Time 36000 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
61600 psi
@Time 10.0 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 435 MPa
@Time 360000 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
63100 psi
@Time 100 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 455 MPa
@Time 3.60e+6 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
66000 psi
@Time 1000 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 455 MPa
@Time 1800 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
66000 psi
@Time 0.500 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 460 MPa
@Time 3.60e+7 sec,
Treatment Temp. 150 °C,
Thickness 70.0 mm
66700 psi
@Time 10000 hour,
Treatment Temp. 302 °F,
Thickness 2.76 in
 460 MPa
@Time 36000 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
66700 psi
@Time 10.0 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 470 MPa
@Time 360000 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
68200 psi
@Time 100 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 470 MPa
@Time 1800 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
68200 psi
@Time 0.500 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 475 MPa
@Time 3.60e+6 sec,
Treatment Temp. 150 °C,
Thickness 70.0 mm
68900 psi
@Time 1000 hour,
Treatment Temp. 302 °F,
Thickness 2.76 in
 475 MPa
@Time 1800 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
68900 psi
@Time 0.500 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 485 MPa
@Time 360 - 3.60e+7 sec,
Treatment Temp. 100 °C,
Thickness 70.0 mm
70300 psi
@Time 0.100 - 10000 hour,
Treatment Temp. 212 °F,
Thickness 2.76 in
 485 MPa
@Time 360 - 36000 sec,
Treatment Temp. 150 °C,
Thickness 70.0 mm
70300 psi
@Time 0.100 - 10.0 hour,
Treatment Temp. 302 °F,
Thickness 2.76 in
 485 MPa
@Time 360000 sec,
Treatment Temp. 150 °C,
Thickness 70.0 mm
70300 psi
@Time 100 hour,
Treatment Temp. 302 °F,
Thickness 2.76 in
 485 MPa
@Time 360 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
70300 psi
@Time 0.100 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 485 MPa
@Time 1800 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
70300 psi
@Time 0.500 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 485 MPa
@Time 36000 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
70300 psi
@Time 10.0 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
Tensile Strength, Yield 441 MPa64000 psiAA; Typical
 420 MPa
@Thickness 38.1 - 50.8 mm
60900 psi
@Thickness 1.50 - 2.00 in
Short transverse
 420 MPa
@Thickness 50.8 - 76.2 mm
60900 psi
@Thickness 2.00 - 3.00 in
Short transverse
 435 MPa
@Thickness 38.1 - 50.8 mm
63100 psi
@Thickness 1.50 - 2.00 in
Long transverse
 435 MPa
@Thickness 50.8 - 76.2 mm
63100 psi
@Thickness 2.00 - 3.00 in
Long transverse
 440 MPa
@Thickness 38.1 - 50.8 mm
63800 psi
@Thickness 1.50 - 2.00 in
Longitudinal
 440 MPa
@Thickness 50.8 - 76.2 mm
63800 psi
@Thickness 2.00 - 3.00 in
Longitudinal
 2.00 MPa
@Thickness 70.0 mm,
Temperature 535 °C
290 psi
@Thickness 2.76 in,
Temperature 995 °F
 12.0 MPa
@Thickness 70.0 mm,
Temperature 480 °C
1740 psi
@Thickness 2.76 in,
Temperature 896 °F
 450 MPa
@Thickness 70.0 mm,
Temperature 24.0 °C
65300 psi
@Thickness 2.76 in,
Temperature 75.2 °F
 470 MPa
@Thickness 70.0 mm,
Temperature -28.0 °C
68200 psi
@Thickness 2.76 in,
Temperature -18.4 °F
 490 MPa
@Thickness 70.0 mm,
Temperature -80.0 °C
71100 psi
@Thickness 2.76 in,
Temperature -112 °F
 545 MPa
@Thickness 70.0 mm,
Temperature -195 °C
79000 psi
@Thickness 2.76 in,
Temperature -319 °F
 620 MPa
@Thickness 70.0 mm,
Temperature -269 °C
89900 psi
@Thickness 2.76 in,
Temperature -452 °F
 24.0 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 425 °C
3480 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 797 °F
 28.0 MPa
@Thickness 70.0 mm,
Temperature 370 °C,
Time 3.60e+6 sec
4060 psi
@Thickness 2.76 in,
Temperature 698 °F,
Time 1000 hour
 28.0 MPa
@Thickness 70.0 mm,
Temperature 370 °C,
Time 3.60e+7 sec
4060 psi
@Thickness 2.76 in,
Temperature 698 °F,
Time 10000 hour
 28.0 MPa
@Thickness 70.0 mm,
Temperature 370 °C,
Time 3.60e+8 sec
4060 psi
@Thickness 2.76 in,
Temperature 698 °F,
Time 100000 hour
 28.0 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 425 °C
4060 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 797 °F
 31.0 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 370 °C
4500 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 698 °F
 34.0 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 370 °C
4930 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 698 °F
 38.0 MPa
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+8 sec
5510 psi
@Thickness 2.76 in,
Temperature 599 °F,
Time 100000 hour
 41.0 MPa
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+7 sec
5950 psi
@Thickness 2.76 in,
Temperature 599 °F,
Time 10000 hour
 45.0 MPa
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+8 sec
6530 psi
@Thickness 2.76 in,
Temperature 500 °F,
Time 100000 hour
 45.0 MPa
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+6 sec
6530 psi
@Thickness 2.76 in,
Temperature 599 °F,
Time 1000 hour
 45.0 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 370 °C
6530 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 698 °F
 55.0 MPa
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+7 sec
7980 psi
@Thickness 2.76 in,
Temperature 500 °F,
Time 10000 hour
 55.0 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 315 °C
7980 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 599 °F
 59.0 MPa
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+8 sec
8560 psi
@Thickness 2.76 in,
Temperature 446 °F,
Time 100000 hour
 69.0 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 315 °C
10000 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 599 °F
 69.0 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 370 °C
10000 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 698 °F
 76.0 MPa
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+7 sec
11000 psi
@Thickness 2.76 in,
Temperature 446 °F,
Time 10000 hour
 76.0 MPa
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+6 sec
11000 psi
@Thickness 2.76 in,
Temperature 500 °F,
Time 1000 hour
 90.0 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+8 sec
13100 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 100000 hour
 115 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 315 °C
16700 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 599 °F
 125 MPa
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+6 sec
18100 psi
@Thickness 2.76 in,
Temperature 446 °F,
Time 1000 hour
 125 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 260 °C
18100 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 500 °F
 140 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+7 sec
20300 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 10000 hour
 145 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 315 °C
21000 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 599 °F
 180 MPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+8 sec
26100 psi
@Thickness 2.76 in,
Temperature 347 °F,
Time 100000 hour
 185 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 260 °C
26800 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 500 °F
 200 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 230 °C
29000 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 446 °F
 220 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+6 sec
31900 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 1000 hour
 230 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 260 °C
33400 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 500 °F
 240 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 260 °C
34800 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 500 °F
 250 MPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+7 sec
36300 psi
@Thickness 2.76 in,
Temperature 347 °F,
Time 10000 hour
 250 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 230 °C
36300 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 446 °F
 270 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 205 °C
39200 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 401 °F
 285 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 230 °C
41300 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 446 °F
 295 MPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+8 sec
42800 psi
@Thickness 2.76 in,
Temperature 302 °F,
Time 100000 hour
 295 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 230 °C
42800 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 446 °F
 305 MPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+6 sec
44200 psi
@Thickness 2.76 in,
Temperature 347 °F,
Time 1000 hour
 310 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 205 °C
45000 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 401 °F
 330 MPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+7 sec
47900 psi
@Thickness 2.76 in,
Temperature 302 °F,
Time 10000 hour
 330 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 205 °C
47900 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 401 °F
 340 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 175 °C
49300 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 347 °F
 340 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 205 °C
49300 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 401 °F
 360 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 175 °C
52200 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 347 °F
 365 MPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 175 °C
52900 psi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 347 °F
 370 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 175 °C
53700 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 347 °F
 380 MPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+6 sec
55100 psi
@Thickness 2.76 in,
Temperature 302 °F,
Time 1000 hour
 395 MPa
@Time 360 - 36000 sec,
Thickness 70.0 mm,
Temperature 150 °C
57300 psi
@Time 0.100 - 10.0 hour,
Thickness 2.76 in,
Temperature 302 °F
 395 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 150 °C
57300 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 302 °F
 415 MPa
@Thickness 70.0 mm,
Temperature 100 °C,
Time 3.60e+8 sec
60200 psi
@Thickness 2.76 in,
Temperature 212 °F,
Time 100000 hour
 420 MPa
@Time 360 - 3.60e+7 sec,
Thickness 70.0 mm,
Temperature 100 °C
60900 psi
@Time 0.100 - 10000 hour,
Thickness 2.76 in,
Temperature 212 °F
 450 MPa
@Treatment Temp. 24.0 °C,
Thickness 70.0 mm
65300 psi
@Treatment Temp. 75.2 °F,
Thickness 2.76 in
 76.0 MPa
@Time 3.60e+7 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
11000 psi
@Time 10000 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 76.0 MPa
@Time 3.60e+7 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
11000 psi
@Time 10000 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 83.0 MPa
@Time 3.60e+7 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
12000 psi
@Time 10000 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 83.0 MPa
@Time 3.60e+6 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
12000 psi
@Time 1000 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 83.0 MPa
@Time 3.60e+6 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
12000 psi
@Time 1000 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 90.0 MPa
@Time 3.60e+7 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
13100 psi
@Time 10000 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 90.0 MPa
@Time 360000 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
13100 psi
@Time 100 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 105 MPa
@Time 360000 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
15200 psi
@Time 100 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 105 MPa
@Time 36000 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
15200 psi
@Time 10.0 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 110 MPa
@Time 3.60e+6 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
16000 psi
@Time 1000 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 130 MPa
@Time 36000 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
18900 psi
@Time 10.0 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 130 MPa
@Time 1800 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
18900 psi
@Time 0.500 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 165 MPa
@Time 3.60e+7 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
23900 psi
@Time 10000 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 170 MPa
@Time 3.60e+6 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
24700 psi
@Time 1000 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 170 MPa
@Time 360000 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
24700 psi
@Time 100 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 230 MPa
@Time 1800 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
33400 psi
@Time 0.500 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 275 MPa
@Time 360000 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
39900 psi
@Time 100 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 295 MPa
@Time 36000 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
42800 psi
@Time 10.0 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 305 MPa
@Time 3.60e+6 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
44200 psi
@Time 1000 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 305 MPa
@Time 3.60e+7 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
44200 psi
@Time 10000 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 360 MPa
@Time 36000 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
52200 psi
@Time 10.0 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 370 MPa
@Time 360000 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
53700 psi
@Time 100 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 400 MPa
@Time 3.60e+6 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
58000 psi
@Time 1000 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 400 MPa
@Time 1800 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
58000 psi
@Time 0.500 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 405 MPa
@Time 3.60e+7 sec,
Treatment Temp. 150 °C,
Thickness 70.0 mm
58700 psi
@Time 10000 hour,
Treatment Temp. 302 °F,
Thickness 2.76 in
 405 MPa
@Time 36000 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
58700 psi
@Time 10.0 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 420 MPa
@Time 360000 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
60900 psi
@Time 100 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 425 MPa
@Time 1800 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
61600 psi
@Time 0.500 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 435 MPa
@Time 3.60e+6 sec,
Treatment Temp. 150 °C,
Thickness 70.0 mm
63100 psi
@Time 1000 hour,
Treatment Temp. 302 °F,
Thickness 2.76 in
 435 MPa
@Time 36000 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
63100 psi
@Time 10.0 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 435 MPa
@Time 1800 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
63100 psi
@Time 0.500 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 440 MPa
@Time 360000 sec,
Treatment Temp. 150 °C,
Thickness 70.0 mm
63800 psi
@Time 100 hour,
Treatment Temp. 302 °F,
Thickness 2.76 in
 450 MPa
@Time 360 - 3.60e+7 sec,
Treatment Temp. 100 °C,
Thickness 70.0 mm
65300 psi
@Time 0.100 - 10000 hour,
Treatment Temp. 212 °F,
Thickness 2.76 in
 450 MPa
@Time 360 - 36000 sec,
Treatment Temp. 150 °C,
Thickness 70.0 mm
65300 psi
@Time 0.100 - 10.0 hour,
Treatment Temp. 302 °F,
Thickness 2.76 in
 450 MPa
@Time 360 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
65300 psi
@Time 0.100 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 450 MPa
@Time 1800 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
65300 psi
@Time 0.500 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
Elongation at Break  4.0 %
@Thickness 50.8 - 76.2 mm
4.0 %
@Thickness 2.00 - 3.00 in
Short transverse
 5.0 %
@Thickness 38.1 - 50.8 mm
5.0 %
@Thickness 1.50 - 2.00 in
Short transverse
 8.0 %
@Thickness 50.8 - 76.2 mm
8.0 %
@Thickness 2.00 - 3.00 in
Long transverse
 9.0 %
@Thickness 38.1 - 50.8 mm
9.0 %
@Thickness 1.50 - 2.00 in
Long transverse
 9.0 %
@Thickness 50.8 - 76.2 mm
9.0 %
@Thickness 2.00 - 3.00 in
Longitudinal
 9.0 %
@Thickness 38.1 - 50.8 mm
9.0 %
@Thickness 1.50 - 2.00 in
Longitudinal
 2.0 %
@Thickness 70.0 mm,
Temperature 535 °C
2.0 %
@Thickness 2.76 in,
Temperature 995 °F
 8.0 %
@Thickness 70.0 mm,
Temperature -80.0 °C
8.0 %
@Thickness 2.76 in,
Temperature -112 °F
 8.0 %
@Thickness 70.0 mm,
Temperature -28.0 °C
8.0 %
@Thickness 2.76 in,
Temperature -18.4 °F
 8.0 %
@Thickness 70.0 mm,
Temperature 24.0 °C
8.0 %
@Thickness 2.76 in,
Temperature 75.2 °F
 9.0 %
@Thickness 70.0 mm,
Temperature -195 °C
9.0 %
@Thickness 2.76 in,
Temperature -319 °F
 10 %
@Thickness 70.0 mm,
Temperature -269 °C
10 %
@Thickness 2.76 in,
Temperature -452 °F
 65 %
@Thickness 70.0 mm,
Temperature 480 °C
65 %
@Thickness 2.76 in,
Temperature 896 °F
 8.0 %
@Diameter 12.7 mm
8.0 %
@Diameter 0.500 in
AA; Typical
 9.0 %
@Time 360 - 3.60e+7 sec,
Thickness 70.0 mm,
Temperature 100 °C
9.0 %
@Time 0.100 - 10000 hour,
Thickness 2.76 in,
Temperature 212 °F
 9.0 %
@Thickness 70.0 mm,
Temperature 100 °C,
Time 3.60e+8 sec
9.0 %
@Thickness 2.76 in,
Temperature 212 °F,
Time 100000 hour
 10 %
@Time 360 - 36000 sec,
Thickness 70.0 mm,
Temperature 150 °C
10 %
@Time 0.100 - 10.0 hour,
Thickness 2.76 in,
Temperature 302 °F
 10 %
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 150 °C
10 %
@Thickness 2.76 in,
Time 100 hour,
Temperature 302 °F
 11 %
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+6 sec
11 %
@Thickness 2.76 in,
Temperature 302 °F,
Time 1000 hour
 12 %
@Time 360 sec,
Thickness 70.0 mm,
Temperature 175 °C
12 %
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 347 °F
 12 %
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 175 °C
12 %
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 347 °F
 12 %
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 175 °C
12 %
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 347 °F
 12 %
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 175 °C
12 %
@Thickness 2.76 in,
Time 100 hour,
Temperature 347 °F
 13 %
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+7 sec
13 %
@Thickness 2.76 in,
Temperature 302 °F,
Time 10000 hour
 13 %
@Time 360 sec,
Thickness 70.0 mm,
Temperature 205 °C
13 %
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 401 °F
 13 %
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 205 °C
13 %
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 401 °F
 14 %
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+6 sec
14 %
@Thickness 2.76 in,
Temperature 347 °F,
Time 1000 hour
 14 %
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 205 °C
14 %
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 401 °F
 15 %
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+8 sec
15 %
@Thickness 2.76 in,
Temperature 302 °F,
Time 100000 hour
 15 %
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 205 °C
15 %
@Thickness 2.76 in,
Time 100 hour,
Temperature 401 °F
 15 %
@Time 360 sec,
Thickness 70.0 mm,
Temperature 230 °C
15 %
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 446 °F
 15 %
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 230 °C
15 %
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 446 °F
 16 %
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+7 sec
16 %
@Thickness 2.76 in,
Temperature 347 °F,
Time 10000 hour
 17 %
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 230 °C
17 %
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 446 °F
 17 %
@Time 360 sec,
Thickness 70.0 mm,
Temperature 260 °C
17 %
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 500 °F
 17 %
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 260 °C
17 %
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 500 °F
 19 %
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+6 sec
19 %
@Thickness 2.76 in,
Temperature 401 °F,
Time 1000 hour
 20 %
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 230 °C
20 %
@Thickness 2.76 in,
Time 100 hour,
Temperature 446 °F
 20 %
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 260 °C
20 %
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 500 °F
 23 %
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+8 sec
23 %
@Thickness 2.76 in,
Temperature 347 °F,
Time 100000 hour
 23 %
@Time 360 sec,
Thickness 70.0 mm,
Temperature 315 °C
23 %
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 599 °F
 26 %
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 315 °C
26 %
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 599 °F
 28 %
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+7 sec
28 %
@Thickness 2.76 in,
Temperature 401 °F,
Time 10000 hour
 29 %
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 260 °C
29 %
@Thickness 2.76 in,
Time 100 hour,
Temperature 500 °F
 30 %
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+6 sec
30 %
@Thickness 2.76 in,
Temperature 446 °F,
Time 1000 hour
 35 %
@Time 360 sec,
Thickness 70.0 mm,
Temperature 370 °C
35 %
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 698 °F
 40 %
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+8 sec
40 %
@Thickness 2.76 in,
Temperature 401 °F,
Time 100000 hour
 40 %
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 315 °C
40 %
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 599 °F
 45 %
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+7 sec
45 %
@Thickness 2.76 in,
Temperature 446 °F,
Time 10000 hour
 45 %
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+6 sec
45 %
@Thickness 2.76 in,
Temperature 500 °F,
Time 1000 hour
 50 %
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 315 °C
50 %
@Thickness 2.76 in,
Time 100 hour,
Temperature 599 °F
 50 %
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 370 °C
50 %
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 698 °F
 55 %
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+8 sec
55 %
@Thickness 2.76 in,
Temperature 446 °F,
Time 100000 hour
 60 %
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+7 sec
60 %
@Thickness 2.76 in,
Temperature 500 °F,
Time 10000 hour
 65 %
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+8 sec
65 %
@Thickness 2.76 in,
Temperature 500 °F,
Time 100000 hour
 65 %
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+6 sec
65 %
@Thickness 2.76 in,
Temperature 599 °F,
Time 1000 hour
 65 %
@Time 360 sec,
Thickness 70.0 mm,
Temperature 425 °C
65 %
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 797 °F
 75 %
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+7 sec
75 %
@Thickness 2.76 in,
Temperature 599 °F,
Time 10000 hour
 75 %
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 370 °C
75 %
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 698 °F
 80 %
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+8 sec
80 %
@Thickness 2.76 in,
Temperature 599 °F,
Time 100000 hour
 85 %
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 370 °C
85 %
@Thickness 2.76 in,
Time 100 hour,
Temperature 698 °F
 85 %
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 425 °C
85 %
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 797 °F
 90 %
@Thickness 70.0 mm,
Temperature 370 °C,
Time 3.60e+6 sec
90 %
@Thickness 2.76 in,
Temperature 698 °F,
Time 1000 hour
 95 %
@Thickness 70.0 mm,
Temperature 370 °C,
Time 3.60e+7 sec
95 %
@Thickness 2.76 in,
Temperature 698 °F,
Time 10000 hour
 100 %
@Thickness 70.0 mm,
Temperature 370 °C,
Time 3.60e+8 sec
100 %
@Thickness 2.76 in,
Temperature 698 °F,
Time 100000 hour
 8.0 %
@Treatment Temp. 24.0 °C,
Thickness 70.0 mm
8.0 %
@Treatment Temp. 75.2 °F,
Thickness 2.76 in
 8.0 %
@Time 360 - 3.60e+7 sec,
Treatment Temp. 100 °C,
Thickness 70.0 mm
8.0 %
@Time 0.100 - 10000 hour,
Treatment Temp. 212 °F,
Thickness 2.76 in
 8.0 %
@Time 360 - 36000 sec,
Treatment Temp. 150 °C,
Thickness 70.0 mm
8.0 %
@Time 0.100 - 10.0 hour,
Treatment Temp. 302 °F,
Thickness 2.76 in
 8.0 %
@Time 360000 sec,
Treatment Temp. 150 °C,
Thickness 70.0 mm
8.0 %
@Time 100 hour,
Treatment Temp. 302 °F,
Thickness 2.76 in
 8.0 %
@Time 3.60e+6 sec,
Treatment Temp. 150 °C,
Thickness 70.0 mm
8.0 %
@Time 1000 hour,
Treatment Temp. 302 °F,
Thickness 2.76 in
 8.0 %
@Time 3.60e+7 sec,
Treatment Temp. 150 °C,
Thickness 70.0 mm
8.0 %
@Time 10000 hour,
Treatment Temp. 302 °F,
Thickness 2.76 in
 8.0 %
@Time 360 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
8.0 %
@Time 0.100 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 8.0 %
@Time 1800 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
8.0 %
@Time 0.500 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 8.0 %
@Time 36000 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
8.0 %
@Time 10.0 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 8.0 %
@Time 360000 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
8.0 %
@Time 100 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 8.0 %
@Time 3.60e+6 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
8.0 %
@Time 1000 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 8.0 %
@Time 1800 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
8.0 %
@Time 0.500 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 8.0 %
@Time 36000 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
8.0 %
@Time 10.0 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 8.0 %
@Time 360000 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
8.0 %
@Time 100 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 8.0 %
@Time 1800 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
8.0 %
@Time 0.500 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 8.0 %
@Time 36000 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
8.0 %
@Time 10.0 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 9.0 %
@Time 3.60e+6 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
9.0 %
@Time 1000 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 9.0 %
@Time 1800 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
9.0 %
@Time 0.500 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 10 %
@Time 3.60e+7 sec,
Treatment Temp. 175 °C,
Thickness 70.0 mm
10 %
@Time 10000 hour,
Treatment Temp. 347 °F,
Thickness 2.76 in
 10 %
@Time 360000 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
10 %
@Time 100 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 10 %
@Time 36000 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
10 %
@Time 10.0 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 10 %
@Time 1800 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
10 %
@Time 0.500 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 12 %
@Time 3.60e+7 sec,
Treatment Temp. 205 °C,
Thickness 70.0 mm
12 %
@Time 10000 hour,
Treatment Temp. 401 °F,
Thickness 2.76 in
 12 %
@Time 3.60e+6 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
12 %
@Time 1000 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 12 %
@Time 360000 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
12 %
@Time 100 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 13 %
@Time 36000 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
13 %
@Time 10.0 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 13 %
@Time 1800 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
13 %
@Time 0.500 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 17 %
@Time 3.60e+6 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
17 %
@Time 1000 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 17 %
@Time 360000 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
17 %
@Time 100 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 18 %
@Time 3.60e+7 sec,
Treatment Temp. 230 °C,
Thickness 70.0 mm
18 %
@Time 10000 hour,
Treatment Temp. 446 °F,
Thickness 2.76 in
 18 %
@Time 36000 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
18 %
@Time 10.0 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 22 %
@Time 3.60e+7 sec,
Treatment Temp. 260 °C,
Thickness 70.0 mm
22 %
@Time 10000 hour,
Treatment Temp. 500 °F,
Thickness 2.76 in
 22 %
@Time 3.60e+6 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
22 %
@Time 1000 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 22 %
@Time 3.60e+7 sec,
Treatment Temp. 315 °C,
Thickness 70.0 mm
22 %
@Time 10000 hour,
Treatment Temp. 599 °F,
Thickness 2.76 in
 22 %
@Time 360000 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
22 %
@Time 100 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 22 %
@Time 3.60e+6 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
22 %
@Time 1000 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
 22 %
@Time 3.60e+7 sec,
Treatment Temp. 370 °C,
Thickness 70.0 mm
22 %
@Time 10000 hour,
Treatment Temp. 698 °F,
Thickness 2.76 in
Creep Strength  18.0 MPa
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+6 sec
2610 psi
@Thickness 2.76 in,
Temperature 599 °F,
Time 1000 hour
0.5% creep
 20.0 MPa
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+6 sec
2900 psi
@Thickness 2.76 in,
Temperature 599 °F,
Time 1000 hour
1% creep
 21.0 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 315 °C
3050 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 599 °F
0.1% creep
 25.0 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 315 °C
3630 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 599 °F
0.2% creep
 30.0 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 315 °C
4350 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 599 °F
0.5% creep
 34.0 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 315 °C
4930 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 599 °F
1% creep
 38.0 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 315 °C
5510 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 599 °F
0.1% creep
 45.0 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 315 °C
6530 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 599 °F
0.2% creep
 52.0 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 315 °C
7540 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 599 °F
0.5% creep
 52.0 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+6 sec
7540 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 1000 hour
0.1% creep
 55.0 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 315 °C
7980 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 599 °F
1% creep
 59.0 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+7 sec
8560 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 10000 hour
0.5% creep
 59.0 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 315 °C
8560 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 599 °F
0.1% creep
 69.0 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+7 sec
10000 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 10000 hour
1% creep
 69.0 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 260 °C
10000 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 500 °F
0.5% creep
 69.0 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 315 °C
10000 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 599 °F
0.2% creep
 76.0 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 260 °C
11000 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 500 °F
1% creep
 76.0 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 260 °C
11000 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 500 °F
0.1% creep
 83.0 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 315 °C
12000 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 599 °F
0.5% creep
 90.0 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 315 °C
13100 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 599 °F
1% creep
 90.0 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+6 sec
13100 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 1000 hour
0.2% creep
 90.0 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 315 °C
13100 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 599 °F
0.1% creep
 97.0 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 260 °C
14100 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 500 °F
0.2% creep
 97.0 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 315 °C
14100 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 599 °F
0.2% creep
 105 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 315 °C
15200 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 599 °F
0.5% creep
 105 MPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+6 sec
15200 psi
@Thickness 2.76 in,
Temperature 347 °F,
Time 1000 hour
0.1% creep
 110 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 315 °C
16000 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 599 °F
1% creep
 115 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+6 sec
16700 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 1000 hour
0.5% creep
 115 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 230 °C
16700 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 446 °F
0.5% creep
 115 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 205 °C
16700 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 401 °F
0.1% creep
 115 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 230 °C
16700 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 446 °F
0.1% creep
 125 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+6 sec
18100 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 1000 hour
1% creep
 125 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 230 °C
18100 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 446 °F
1% creep
 125 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 260 °C
18100 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 500 °F
0.5% creep
 130 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 260 °C
18900 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 500 °F
1% creep
 130 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 260 °C
18900 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 500 °F
0.1% creep
 140 MPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+6 sec
20300 psi
@Thickness 2.76 in,
Temperature 347 °F,
Time 1000 hour
0.2% creep
 150 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 205 °C
21800 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 401 °F
0.2% creep
 150 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 230 °C
21800 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 446 °F
0.2% creep
 150 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 260 °C
21800 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 500 °F
0.2% creep
 170 MPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+6 sec
24700 psi
@Thickness 2.76 in,
Temperature 347 °F,
Time 1000 hour
0.5% creep
 170 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 260 °C
24700 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 500 °F
0.5% creep
 170 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 175 °C
24700 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 347 °F
0.1% creep
 170 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 205 °C
24700 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 401 °F
0.1% creep
 170 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 230 °C
24700 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 446 °F
0.1% creep
 170 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 260 °C
24700 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 500 °F
0.1% creep
 180 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 260 °C
26100 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 500 °F
1% creep
 180 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 205 °C
26100 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 401 °F
0.5% creep
 180 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 230 °C
26100 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 446 °F
0.5% creep
 180 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 260 °C
26100 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 500 °F
0.2% creep
 185 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 205 °C
26800 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 401 °F
1% creep
 185 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 230 °C
26800 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 446 °F
1% creep
 195 MPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+6 sec
28300 psi
@Thickness 2.76 in,
Temperature 347 °F,
Time 1000 hour
1% creep
 200 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 260 °C
29000 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 500 °F
0.5% creep
 205 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 260 °C
29700 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 500 °F
1% creep
 205 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 175 °C
29700 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 347 °F
0.2% creep
 205 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 205 °C
29700 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 401 °F
0.2% creep
 205 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 230 °C
29700 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 446 °F
0.2% creep
 205 MPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+6 sec
29700 psi
@Thickness 2.76 in,
Temperature 302 °F,
Time 1000 hour
0.1% creep
 215 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 230 °C
31200 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 446 °F
0.1% creep
 220 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 230 °C
31900 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 446 °F
0.5% creep
 220 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 205 °C
31900 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 401 °F
0.1% creep
 230 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 175 °C
33400 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 347 °F
0.1% creep
 235 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 230 °C
34100 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 446 °F
1% creep
 235 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 205 °C
34100 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 401 °F
0.5% creep
 235 MPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+6 sec
34100 psi
@Thickness 2.76 in,
Temperature 302 °F,
Time 1000 hour
0.2% creep
 235 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 230 °C
34100 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 446 °F
0.2% creep
 240 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 205 °C
34800 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 401 °F
1% creep
 240 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 175 °C
34800 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 347 °F
0.5% creep
 250 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 230 °C
36300 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 446 °F
0.5% creep
 250 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 205 °C
36300 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 401 °F
0.2% creep
 250 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 150 °C
36300 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 302 °F
0.1% creep
 255 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 175 °C
37000 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 347 °F
1% creep
 255 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 175 °C
37000 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 347 °F
0.2% creep
 260 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 230 °C
37700 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 446 °F
1% creep
 260 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 175 °C
37700 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 347 °F
0.1% creep
 260 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 205 °C
37700 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 401 °F
0.1% creep
 270 MPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+6 sec
39200 psi
@Thickness 2.76 in,
Temperature 302 °F,
Time 1000 hour
0.5% creep
 270 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 205 °C
39200 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 401 °F
0.5% creep
 275 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 205 °C
39900 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 401 °F
1% creep
 275 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 175 °C
39900 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 347 °F
0.5% creep
 285 MPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+6 sec
41300 psi
@Thickness 2.76 in,
Temperature 302 °F,
Time 1000 hour
1% creep
 285 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 205 °C
41300 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 401 °F
0.2% creep
 285 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 150 °C
41300 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 302 °F
0.1% creep
 290 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 175 °C
42100 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 347 °F
1% creep
 290 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 150 °C
42100 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 302 °F
0.2% creep
 290 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 175 °C
42100 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 347 °F
0.2% creep
 295 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 205 °C
42800 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 401 °F
0.5% creep
 305 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 150 °C
44200 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 302 °F
0.5% creep
 305 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 175 °C
44200 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 347 °F
0.1% creep
 310 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 150 °C
45000 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 302 °F
1% creep
 310 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 205 °C
45000 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 401 °F
1% creep
 310 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 175 °C
45000 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 347 °F
0.5% creep
 310 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 150 °C
45000 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 302 °F
0.2% creep
 310 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 150 °C
45000 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 302 °F
0.1% creep
 325 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 175 °C
47100 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 347 °F
1% creep
 325 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 150 °C
47100 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 302 °F
0.5% creep
 325 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 175 °C
47100 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 347 °F
0.2% creep
 325 MPa
@Thickness 70.0 mm,
Temperature 100 °C,
Time 3.60e+6 sec
47100 psi
@Thickness 2.76 in,
Temperature 212 °F,
Time 1000 hour
0.1% creep
 330 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 150 °C
47900 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 302 °F
0.2% creep
 340 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 150 °C
49300 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 302 °F
1% creep
 340 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 175 °C
49300 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 347 °F
0.5% creep
 340 MPa
@Thickness 70.0 mm,
Temperature 100 °C,
Time 3.60e+6 sec
49300 psi
@Thickness 2.76 in,
Temperature 212 °F,
Time 1000 hour
0.2% creep
 345 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 175 °C
50000 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 347 °F
1% creep
 345 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 150 °C
50000 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 302 °F
0.5% creep
 345 MPa
@Thickness 70.0 mm,
Temperature 100 °C,
Time 360000 sec
50000 psi
@Thickness 2.76 in,
Temperature 212 °F,
Time 100 hour
0.1% creep
 345 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 150 °C
50000 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 302 °F
0.1% creep
 360 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 150 °C
52200 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 302 °F
1% creep
 360 MPa
@Thickness 70.0 mm,
Temperature 100 °C,
Time 3.60e+6 sec
52200 psi
@Thickness 2.76 in,
Temperature 212 °F,
Time 1000 hour
0.5% creep
 360 MPa
@Thickness 70.0 mm,
Temperature 100 °C,
Time 360000 sec
52200 psi
@Thickness 2.76 in,
Temperature 212 °F,
Time 100 hour
0.2% creep
 360 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 150 °C
52200 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 302 °F
0.2% creep
 370 MPa
@Thickness 70.0 mm,
Temperature 100 °C,
Time 3.60e+6 sec
53700 psi
@Thickness 2.76 in,
Temperature 212 °F,
Time 1000 hour
1% creep
 370 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 150 °C
53700 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 302 °F
0.5% creep
 370 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 100 °C
53700 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 212 °F
0.1% creep
 380 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 150 °C
55100 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 302 °F
1% creep
 380 MPa
@Thickness 70.0 mm,
Temperature 100 °C,
Time 360000 sec
55100 psi
@Thickness 2.76 in,
Temperature 212 °F,
Time 100 hour
0.5% creep
 380 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 100 °C
55100 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 212 °F
0.2% creep
 385 MPa
@Thickness 70.0 mm,
Temperature 100 °C,
Time 360000 sec
55800 psi
@Thickness 2.76 in,
Temperature 212 °F,
Time 100 hour
1% creep
 395 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 100 °C
57300 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 212 °F
0.5% creep
 395 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 100 °C
57300 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 212 °F
0.1% creep
 405 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 100 °C
58700 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 212 °F
1% creep
 405 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 100 °C
58700 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 212 °F
0.2% creep
 415 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 100 °C
60200 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 212 °F
0.5% creep
 415 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 100 °C
60200 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 212 °F
0.1% creep
 420 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 100 °C
60900 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 212 °F
1% creep
 420 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 100 °C
60900 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 212 °F
0.2% creep
 425 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 100 °C
61600 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 212 °F
0.5% creep
 435 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 100 °C
63100 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 212 °F
1% creep
 450 MPa
@Time 3600 sec,
Temperature 24.0 °C,
Thickness 70.0 mm
65300 psi
@Time 1.00 hour,
Temperature 75.2 °F,
Thickness 2.76 in
0.5% creep
 455 MPa
@Time 36000 sec,
Temperature 24.0 °C,
Thickness 70.0 mm
66000 psi
@Time 10.0 hour,
Temperature 75.2 °F,
Thickness 2.76 in
1% creep
 455 MPa
@Time 360 sec,
Temperature 24.0 °C,
Thickness 70.0 mm
66000 psi
@Time 0.100 hour,
Temperature 75.2 °F,
Thickness 2.76 in
0.5% creep
 460 MPa
@Time 3600 sec,
Temperature 24.0 °C,
Thickness 70.0 mm
66700 psi
@Time 1.00 hour,
Temperature 75.2 °F,
Thickness 2.76 in
1% creep
 470 MPa
@Time 360 sec,
Temperature 24.0 °C,
Thickness 70.0 mm
68200 psi
@Time 0.100 hour,
Temperature 75.2 °F,
Thickness 2.76 in
1% creep
Rupture Strength  21.0 MPa
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+6 sec
3050 psi
@Thickness 2.76 in,
Temperature 599 °F,
Time 1000 hour
 23.0 MPa
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+8 sec
3340 psi
@Thickness 2.76 in,
Temperature 500 °F,
Time 100000 hour
 32.0 MPa
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+7 sec
4640 psi
@Thickness 2.76 in,
Temperature 500 °F,
Time 10000 hour
 34.0 MPa
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+8 sec
4930 psi
@Thickness 2.76 in,
Temperature 446 °F,
Time 100000 hour
 34.0 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 315 °C
4930 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 599 °F
 48.0 MPa
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+7 sec
6960 psi
@Thickness 2.76 in,
Temperature 446 °F,
Time 10000 hour
 48.0 MPa
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+6 sec
6960 psi
@Thickness 2.76 in,
Temperature 500 °F,
Time 1000 hour
 52.0 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+8 sec
7540 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 100000 hour
 59.0 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 315 °C
8560 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 599 °F
 76.0 MPa
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+6 sec
11000 psi
@Thickness 2.76 in,
Temperature 446 °F,
Time 1000 hour
 83.0 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+7 sec
12000 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 10000 hour
 83.0 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 260 °C
12000 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 500 °F
 90.0 MPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+8 sec
13100 psi
@Thickness 2.76 in,
Temperature 347 °F,
Time 100000 hour
 97.0 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 315 °C
14100 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 599 °F
 110 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 315 °C
16000 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 599 °F
 130 MPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+6 sec
18900 psi
@Thickness 2.76 in,
Temperature 401 °F,
Time 1000 hour
 130 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 230 °C
18900 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 446 °F
 140 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 260 °C
20300 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 500 °F
 145 MPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+7 sec
21000 psi
@Thickness 2.76 in,
Temperature 347 °F,
Time 10000 hour
 170 MPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+8 sec
24700 psi
@Thickness 2.76 in,
Temperature 302 °F,
Time 100000 hour
 185 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 260 °C
26800 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 500 °F
 195 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 230 °C
28300 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 446 °F
 200 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 205 °C
29000 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 401 °F
 205 MPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+6 sec
29700 psi
@Thickness 2.76 in,
Temperature 347 °F,
Time 1000 hour
 215 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 260 °C
31200 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 500 °F
 235 MPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+7 sec
34100 psi
@Thickness 2.76 in,
Temperature 302 °F,
Time 10000 hour
 240 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 230 °C
34800 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 446 °F
 255 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 205 °C
37000 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 401 °F
 270 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 175 °C
39200 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 347 °F
 275 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 230 °C
39900 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 446 °F
 290 MPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+6 sec
42100 psi
@Thickness 2.76 in,
Temperature 302 °F,
Time 1000 hour
 290 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 205 °C
42100 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 401 °F
 305 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 175 °C
44200 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 347 °F
 315 MPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 150 °C
45700 psi
@Thickness 2.76 in,
Time 100 hour,
Temperature 302 °F
 325 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 205 °C
47100 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 401 °F
 340 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 175 °C
49300 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 347 °F
 345 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 150 °C
50000 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 302 °F
 365 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 175 °C
52900 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 347 °F
 370 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 150 °C
53700 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 302 °F
 380 MPa
@Thickness 70.0 mm,
Temperature 100 °C,
Time 3.60e+6 sec
55100 psi
@Thickness 2.76 in,
Temperature 212 °F,
Time 1000 hour
 400 MPa
@Thickness 70.0 mm,
Temperature 100 °C,
Time 360000 sec
58000 psi
@Thickness 2.76 in,
Temperature 212 °F,
Time 100 hour
 400 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 150 °C
58000 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 302 °F
 420 MPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 100 °C
60900 psi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 212 °F
 435 MPa
@Time 3600 sec,
Thickness 70.0 mm,
Temperature 100 °C
63100 psi
@Time 1.00 hour,
Thickness 2.76 in,
Temperature 212 °F
 455 MPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 100 °C
66000 psi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 212 °F
 470 MPa
@Temperature 24.0 °C,
Thickness 70.0 mm,
Time 360000 sec
68200 psi
@Temperature 75.2 °F,
Thickness 2.76 in,
Time 100 hour
 470 MPa
@Temperature 24.0 °C,
Thickness 70.0 mm,
Time 3.60e+6 sec
68200 psi
@Temperature 75.2 °F,
Thickness 2.76 in,
Time 1000 hour
 475 MPa
@Time 3600 sec,
Temperature 24.0 °C,
Thickness 70.0 mm
68900 psi
@Time 1.00 hour,
Temperature 75.2 °F,
Thickness 2.76 in
 475 MPa
@Time 36000 sec,
Temperature 24.0 °C,
Thickness 70.0 mm
68900 psi
@Time 10.0 hour,
Temperature 75.2 °F,
Thickness 2.76 in
 485 MPa
@Time 360 sec,
Temperature 24.0 °C,
Thickness 70.0 mm
70300 psi
@Time 0.100 hour,
Temperature 75.2 °F,
Thickness 2.76 in
Modulus of Elasticity 73.1 GPa10600 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
 72.0 GPa
@Thickness 70.0 mm,
Temperature 24.0 °C
10400 ksi
@Thickness 2.76 in,
Temperature 75.2 °F
 74.0 GPa
@Thickness 70.0 mm,
Temperature -28.0 °C
10700 ksi
@Thickness 2.76 in,
Temperature -18.4 °F
 76.0 GPa
@Thickness 70.0 mm,
Temperature -80.0 °C
11000 ksi
@Thickness 2.76 in,
Temperature -112 °F
 81.0 GPa
@Thickness 70.0 mm,
Temperature -195 °C
11700 ksi
@Thickness 2.76 in,
Temperature -319 °F
 45.0 GPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 370 °C
6530 ksi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 698 °F
 45.0 GPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 370 °C
6530 ksi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 698 °F
 45.0 GPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 370 °C
6530 ksi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 698 °F
 45.0 GPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 370 °C
6530 ksi
@Thickness 2.76 in,
Time 100 hour,
Temperature 698 °F
 45.0 GPa
@Thickness 70.0 mm,
Temperature 370 °C,
Time 3.60e+6 sec
6530 ksi
@Thickness 2.76 in,
Temperature 698 °F,
Time 1000 hour
 45.0 GPa
@Thickness 70.0 mm,
Temperature 370 °C,
Time 3.60e+7 sec
6530 ksi
@Thickness 2.76 in,
Temperature 698 °F,
Time 10000 hour
 45.0 GPa
@Thickness 70.0 mm,
Temperature 370 °C,
Time 3.60e+8 sec
6530 ksi
@Thickness 2.76 in,
Temperature 698 °F,
Time 100000 hour
 53.0 GPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 315 °C
7690 ksi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 599 °F
 53.0 GPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 315 °C
7690 ksi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 599 °F
 53.0 GPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 315 °C
7690 ksi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 599 °F
 53.0 GPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 315 °C
7690 ksi
@Thickness 2.76 in,
Time 100 hour,
Temperature 599 °F
 53.0 GPa
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+6 sec
7690 ksi
@Thickness 2.76 in,
Temperature 599 °F,
Time 1000 hour
 53.0 GPa
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+7 sec
7690 ksi
@Thickness 2.76 in,
Temperature 599 °F,
Time 10000 hour
 53.0 GPa
@Thickness 70.0 mm,
Temperature 315 °C,
Time 3.60e+8 sec
7690 ksi
@Thickness 2.76 in,
Temperature 599 °F,
Time 100000 hour
 59.0 GPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 260 °C
8560 ksi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 500 °F
 59.0 GPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 260 °C
8560 ksi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 500 °F
 59.0 GPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 260 °C
8560 ksi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 500 °F
 59.0 GPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 260 °C
8560 ksi
@Thickness 2.76 in,
Time 100 hour,
Temperature 500 °F
 59.0 GPa
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+6 sec
8560 ksi
@Thickness 2.76 in,
Temperature 500 °F,
Time 1000 hour
 59.0 GPa
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+7 sec
8560 ksi
@Thickness 2.76 in,
Temperature 500 °F,
Time 10000 hour
 59.0 GPa
@Thickness 70.0 mm,
Temperature 260 °C,
Time 3.60e+8 sec
8560 ksi
@Thickness 2.76 in,
Temperature 500 °F,
Time 100000 hour
 61.0 GPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 230 °C
8850 ksi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 446 °F
 61.0 GPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 230 °C
8850 ksi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 446 °F
 61.0 GPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 230 °C
8850 ksi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 446 °F
 61.0 GPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 230 °C
8850 ksi
@Thickness 2.76 in,
Time 100 hour,
Temperature 446 °F
 61.0 GPa
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+6 sec
8850 ksi
@Thickness 2.76 in,
Temperature 446 °F,
Time 1000 hour
 61.0 GPa
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+7 sec
8850 ksi
@Thickness 2.76 in,
Temperature 446 °F,
Time 10000 hour
 61.0 GPa
@Thickness 70.0 mm,
Temperature 230 °C,
Time 3.60e+8 sec
8850 ksi
@Thickness 2.76 in,
Temperature 446 °F,
Time 100000 hour
 63.0 GPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 205 °C
9140 ksi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 401 °F
 63.0 GPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 205 °C
9140 ksi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 401 °F
 63.0 GPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 205 °C
9140 ksi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 401 °F
 63.0 GPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 205 °C
9140 ksi
@Thickness 2.76 in,
Time 100 hour,
Temperature 401 °F
 63.0 GPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+6 sec
9140 ksi
@Thickness 2.76 in,
Temperature 401 °F,
Time 1000 hour
 63.0 GPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+7 sec
9140 ksi
@Thickness 2.76 in,
Temperature 401 °F,
Time 10000 hour
 63.0 GPa
@Thickness 70.0 mm,
Temperature 205 °C,
Time 3.60e+8 sec
9140 ksi
@Thickness 2.76 in,
Temperature 401 °F,
Time 100000 hour
 66.0 GPa
@Time 360 sec,
Thickness 70.0 mm,
Temperature 175 °C
9570 ksi
@Time 0.100 hour,
Thickness 2.76 in,
Temperature 347 °F
 66.0 GPa
@Time 1800 sec,
Thickness 70.0 mm,
Temperature 175 °C
9570 ksi
@Time 0.500 hour,
Thickness 2.76 in,
Temperature 347 °F
 66.0 GPa
@Time 36000 sec,
Thickness 70.0 mm,
Temperature 175 °C
9570 ksi
@Time 10.0 hour,
Thickness 2.76 in,
Temperature 347 °F
 66.0 GPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 175 °C
9570 ksi
@Thickness 2.76 in,
Time 100 hour,
Temperature 347 °F
 66.0 GPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+6 sec
9570 ksi
@Thickness 2.76 in,
Temperature 347 °F,
Time 1000 hour
 66.0 GPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+7 sec
9570 ksi
@Thickness 2.76 in,
Temperature 347 °F,
Time 10000 hour
 66.0 GPa
@Thickness 70.0 mm,
Temperature 175 °C,
Time 3.60e+8 sec
9570 ksi
@Thickness 2.76 in,
Temperature 347 °F,
Time 100000 hour
 68.0 GPa
@Time 360 - 36000 sec,
Thickness 70.0 mm,
Temperature 150 °C
9860 ksi
@Time 0.100 - 10.0 hour,
Thickness 2.76 in,
Temperature 302 °F
 68.0 GPa
@Thickness 70.0 mm,
Time 360000 sec,
Temperature 150 °C
9860 ksi
@Thickness 2.76 in,
Time 100 hour,
Temperature 302 °F
 68.0 GPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+6 sec
9860 ksi
@Thickness 2.76 in,
Temperature 302 °F,
Time 1000 hour
 68.0 GPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+7 sec
9860 ksi
@Thickness 2.76 in,
Temperature 302 °F,
Time 10000 hour
 68.0 GPa
@Thickness 70.0 mm,
Temperature 150 °C,
Time 3.60e+8 sec
9860 ksi
@Thickness 2.76 in,
Temperature 302 °F,
Time 100000 hour
 71.0 GPa
@Time 360 - 3.60e+7 sec,
Thickness 70.0 mm,
Temperature 100 °C
10300 ksi
@Time 0.100 - 10000 hour,
Thickness 2.76 in,
Temperature 212 °F
 71.0 GPa
@Thickness 70.0 mm,
Temperature 100 °C,
Time 3.60e+8 sec
10300 ksi
@Thickness 2.76 in,
Temperature 212 °F,
Time 100000 hour
Tensile Modulus  55.0 GPa
@Temperature 260 °C
7980 ksi
@Temperature 500 °F
 56.0 GPa
@Temperature 250 °C
8120 ksi
@Temperature 482 °F
 61.0 GPa
@Temperature 200 °C
8850 ksi
@Temperature 392 °F
 65.0 GPa
@Temperature 150 °C
9430 ksi
@Temperature 302 °F
 68.0 GPa
@Temperature 100 °C
9860 ksi
@Temperature 212 °F
 71.0 GPa
@Temperature 50.0 °C
10300 ksi
@Temperature 122 °F
 72.0 GPa
@Temperature 25.0 °C
10400 ksi
@Temperature 77.0 °F
Poissons Ratio 0.330.33Estimated from trends in similar Al alloys.
Fatigue Strength 125 MPa
@# of Cycles 5.00e+8
18100 psi
@# of Cycles 5.00e+8
Fracture Toughness 26.0 MPa-m½23.7 ksi-in½K(IC) in S-L Direction
 26.0 MPa-m½23.7 ksi-in½K(IC) in T-L Direction
 32.0 MPa-m½29.1 ksi-in½K(IC) in L-T Direction
Machinability 70 %70 %0-100 Scale of Aluminum Alloys
Shear Modulus 27.0 GPa3920 ksiEstimated from similar Al alloys.
Shear Strength 295 MPa42800 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000449 ohm-cm
@Temperature 20.0 °C
0.00000449 ohm-cm
@Temperature 68.0 °F
AA; Typical
 
Thermal PropertiesMetricEnglishComments
CTE, linear  21.1 µm/m-°C
@Temperature -50.0 - 20.0 °C
11.7 µin/in-°F
@Temperature -58.0 - 68.0 °F
 22.9 µm/m-°C
@Temperature 20.0 - 100 °C
12.7 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 23.8 µm/m-°C
@Temperature 20.0 - 200 °C
13.2 µin/in-°F
@Temperature 68.0 - 392 °F
 24.7 µm/m-°C
@Temperature 20.0 - 300 °C
13.7 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.882 J/g-°C0.211 BTU/lb-°F
Thermal Conductivity 151 W/m-K1050 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 502 - 638 °C935 - 1180 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 502 °C935 °FAA; Typical
Liquidus 638 °C1180 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 413 °C775 °F
Solution Temperature 493 °C920 °F
Aging Temperature 191 °C375 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 91.2 - 94.7 %91.2 - 94.7 %As remainder
Chromium, Cr <= 0.10 %<= 0.10 %
Copper, Cu 3.8 - 4.9 %3.8 - 4.9 %
Iron, Fe <= 0.30 %<= 0.30 %
Magnesium, Mg 1.2 - 1.8 %1.2 - 1.8 %
Manganese, Mn 0.30 - 0.90 %0.30 - 0.90 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.20 %<= 0.20 %
Titanium, Ti <= 0.15 %<= 0.15 %
Zinc, Zn <= 0.25 %<= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 2124-T851
Aluminum 2124-O
Aluminum 2124-T351
Aluminum 6013-T651
Aluminum 6013-T8

MA2124T851 / 170630

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.