MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

HP Alloys Alloy 718, 0% Cold Worked, Not Aged
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: 0% Cold Worked, Not Aged applies to tensile and/or hardness; other properties are typical of this alloy.

Data provided by High Performance Alloys, Inc., Allvac, Inco Alloys International, and Haynes International.

Key Words: NACE MR-01-75, ASTM B626; AFNOR NC 19 Fe Nb, UNS N07718, AMS 5596, AMS 5597, AMS 5662, AMS 5664, AMS 5832, AMS 5589, AMS 5590, Werkstoff Nr. 2.4668; WL Nr. 2.4668; MIL-N-24469; NACE MR-01-75; AECMA Pr EN 2404, 2405, 2407, 2408, 2952, 2961, 3219
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.20 g/cc0.296 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 862 MPa125000 psi
Tensile Strength, Yield 414 MPa60000 psi
Elongation at Break 51 %51 %
Reduction of Area 63 %63 %
Modulus of Elasticity 200 GPa29000 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000123 ohm-cm0.000123 ohm-cm
Magnetic Permeability 1.00111.0011at 200 Oersted (15.9 kA/m)
Curie Temperature -112 °C-170 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.9 µm/m-°C
@Temperature 20.0 - 100 °C
7.17 µin/in-°F
@Temperature 68.0 - 212 °F
 13.5 µm/m-°C
@Temperature 25.0 - 200 °C
7.50 µin/in-°F
@Temperature 77.0 - 392 °F
 14.3 µm/m-°C
@Temperature 25.0 - 500 °C
7.94 µin/in-°F
@Temperature 77.0 - 932 °F
 17.2 µm/m-°C
@Temperature 25.0 - 900 °C
9.56 µin/in-°F
@Temperature 77.0 - 1650 °F
Specific Heat Capacity 0.435 J/g-°C0.104 BTU/lb-°F
Thermal Conductivity 11.4 W/m-K79.1 BTU-in/hr-ft²-°F
Melting Point 1260 - 1336 °C2300 - 2437 °F
Solidus 1260 °C2300 °F
Liquidus 1336 °C2437 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 0.20 - 0.80 %0.20 - 0.80 %
Boron, B <= 0.0060 %<= 0.0060 %
Carbon, C <= 0.080 %<= 0.080 %
Chromium, Cr 17 - 21 %17 - 21 %
Cobalt, Co <= 1.0 %<= 1.0 %
Copper, Cu <= 0.30 %<= 0.30 %
Iron, Fe 17 %17 %
Manganese, Mn <= 0.35 %<= 0.35 %
Molybdenum, Mo 2.8 - 3.3 %2.8 - 3.3 %
Nickel, Ni 50 - 55 %50 - 55 %
Niobium, Nb (Columbium, Cb) 4.75 - 5.5 %4.75 - 5.5 %
Phosphorus, P <= 0.015 %<= 0.015 %
Silicon, Si <= 0.35 %<= 0.35 %
Sulfur, S <= 0.015 %<= 0.015 %
Titanium, Ti 0.65 - 1.15 %0.65 - 1.15 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
HP Alloys Alloy 718, 5% Cold Worked
Haynes 718 alloy, cold rolled, solution-treated and aged sheet
Special Metals INCONEL® Alloy 718
HP Alloys Alloy 718, 50% Cold Worked
HP Alloys Alloy 718, 5% Cold Worked, Aged

NPH710 / 18787

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.