MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Epoxy Adhesive
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Epoxy Adhesive". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Master Bond is a leading manufacturer of high performance epoxy adhesives, sealants, coatings, potting/encapsulation compounds and impregnation resins. Our epoxies include one and two part formulations that can be cured at room temperature, with heat or exposure to UV light. Special formulations feature high electrical and/or thermal conductivity and wide service temperature ranges. Visit www.masterbond.com.

Kohesi Bond is a pioneer in manufacturing over 300 grades of custom engineered adhesives, sealants, coatings, potting and encapsulation compounds. Our first-rate adhesives are tailor-fitted to meet your exact specifications and offer superior strength and performance in your application. Learn more about Kohesi Bond’s industry-ready products at kohesibond.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 0.137 - 4.80 g/cc0.00494 - 0.173 lb/in³Average value: 1.41 g/cc Grade Count:507
 0.620 - 0.620 g/cc
@Temperature 50.0 - 50.0 °C
0.0224 - 0.0224 lb/in³
@Temperature 122 - 122 °F
Average value: 0.620 g/cc Grade Count:1
Filler Content 20.0 - 61.0 %20.0 - 61.0 %Average value: 32.5 % Grade Count:8
Volatile Organic Compounds (VOC) Content 0.000 - 258 g/l0.000 - 258 g/lAverage value: 96.8 g/l Grade Count:12
Water Absorption 0.00400 - 4.65 %0.00400 - 4.65 %Average value: 0.531 % Grade Count:92
Particle Size 20.0 - 50.0 µm20.0 - 50.0 µmAverage value: 32.0 µm Grade Count:5
Viscosity 0.0100 - 2.50e+7 cP0.0100 - 2.50e+7 cPAverage value: 119000 cP Grade Count:765
 50.0 - 500000 cP
@Temperature 10.0 - 93.3 °C
50.0 - 500000 cP
@Temperature 50.0 - 200 °F
Average value: 60000 cP Grade Count:39
Linear Mold Shrinkage 0.000100 - 0.0100 cm/cm0.000100 - 0.0100 in/inAverage value: 0.00419 cm/cm Grade Count:28
Outgassing - Total Mass Loss 0.0700 - 1.74 %0.0700 - 1.74 %Average value: 0.747 % Grade Count:19
 0.600 - 0.600 %
@Temperature 65.0 - 65.0 °C
0.600 - 0.600 %
@Temperature 149 - 149 °F
Average value: 0.600 % Grade Count:1
 0.600 - 0.600 %
@Time 10800 - 10800 sec
0.600 - 0.600 %
@Time 3.00 - 3.00 hour
Average value: 0.600 % Grade Count:1
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 5.00 - 95.05.00 - 95.0Average value: 62.8 Grade Count:14
Hardness, Shore D 12.0 - 10012.0 - 100Average value: 76.6 Grade Count:667
 24.0 - 88.0
@Temperature -5.56 - 168 °C
24.0 - 88.0
@Temperature 22.0 - 334 °F
Average value: 59.5 Grade Count:13
Tensile Strength, Ultimate 0.276 - 766 MPa40.0 - 111000 psiAverage value: 42.9 MPa Grade Count:564
 0.861845 - 64.8107 MPa
@Temperature -59.0 - 177 °C
125.000 - 9400.02 psi
@Temperature -74.2 - 351 °F
Average value: 9.47 MPa Grade Count:18
Tensile Strength, Yield 1.38 - 40.0 MPa200 - 5800 psiAverage value: 14.8 MPa Grade Count:50
 4.55054 - 8.99766 MPa
@Temperature -55.0 - 177 °C
660.001 - 1305.00 psi
@Temperature -67.0 - 350 °F
Average value: 6.30 MPa Grade Count:7
Elongation at Break 0.000 - 250 %0.000 - 250 %Average value: 16.9 % Grade Count:286
 0.730 - 1.78 %
@Temperature 65.6 - 177 °C
0.730 - 1.78 %
@Temperature 150 - 350 °F
Average value: 1.21 % Grade Count:1
Elongation at Yield 0.700 - 10.0 %0.700 - 10.0 %Average value: 5.56 % Grade Count:6
Modulus of Elasticity 0.0345 - 59.1 GPa5.00 - 8570 ksiAverage value: 3.29 GPa Grade Count:344
 1.37895 - 9.65266 GPa
@Temperature 65.6 - 260 °C
200.003 - 1400.02 ksi
@Temperature 150 - 500 °F
Average value: 3.45 GPa Grade Count:8
Flexural Yield Strength 4.21 - 970 MPa610 - 141000 psiAverage value: 128 MPa Grade Count:57
 17.2369 - 88.2529 MPa
@Temperature 23.9 - 260 °C
2500.00 - 12800.0 psi
@Temperature 75.0 - 500 °F
Average value: 45.8 MPa Grade Count:4
Flexural Modulus 0.103 - 54.4 GPa15.0 - 7890 ksiAverage value: 10.9 GPa Grade Count:17
 3.93001 - 8.06687 GPa
@Temperature 65.6 - 177 °C
570.009 - 1170.02 ksi
@Temperature 150 - 350 °F
Average value: 6.11 GPa Grade Count:1
Compressive Yield Strength 3.45 - 694 MPa500 - 101000 psiAverage value: 106 MPa Grade Count:212
 3.44738 - 173 MPa
@Temperature -55.0 - 177 °C
500.001 - 25100 psi
@Temperature -67.0 - 351 °F
Average value: 28.7 MPa Grade Count:5
Compressive Modulus 0.0414 - 200 GPa6.00 - 29000 ksiAverage value: 8.46 GPa Grade Count:52
Poissons Ratio 0.0200 - 0.6800.0200 - 0.680Average value: 0.321 Grade Count:5
Shear Modulus 0.342 - 5.18 GPa49.6 - 751 ksiAverage value: 1.96 GPa Grade Count:5
 1.50857 - 2.74411 GPa
@Temperature -100 - 0.000 °C
218.803 - 398.006 ksi
@Temperature -148 - 32.0 °F
Average value: 2.10 GPa Grade Count:3
Shear Strength 0.172 - 138 MPa25.0 - 20000 psiAverage value: 18.9 MPa Grade Count:280
 0.151685 - 214.358 MPa
@Temperature -253 - 316 °C
22.0000 - 31090.1 psi
@Temperature -423 - 601 °F
Average value: 17.0 MPa Grade Count:120
 1.37895 - 29.6475 MPa
@Temperature -55.0 - 149 °C
200.000 - 4300.01 psi
@Temperature -67.0 - 300 °F
Average value: 17.0 MPa Grade Count:15
 1.37895 - 29.6475 MPa
@Time 0.000 - 4.41e+6 sec
200.000 - 4300.01 psi
@Time 0.000 - 1220 hour
Average value: 17.0 MPa Grade Count:15
Adhesive Bond Strength 0.621 - 110 MPa90.0 - 16000 psiAverage value: 19.0 MPa Grade Count:566
 3.50 - 48.3 MPa
@Temperature -55.0 - 275 °C
508 - 7010 psi
@Temperature -67.0 - 527 °F
Average value: 17.5 MPa Grade Count:107
 1.17211 - 27.579 MPa
@Temperature 65.0 - 65.0 °C
170.000 - 4000.0 psi
@Temperature 149 - 149 °F
Average value: 17.5 MPa Grade Count:3
 1.17211 - 27.579 MPa
@Time 3600 - 14400 sec
170.000 - 4000.0 psi
@Time 1.00 - 4.00 hour
Average value: 17.5 MPa Grade Count:3
Izod Impact, Notched 0.107 - 2.14 J/cm0.200 - 4.00 ft-lb/inAverage value: 0.797 J/cm Grade Count:25
Gardner Impact 11.0 - 36.2 J8.11 - 26.7 ft-lbAverage value: 21.7 J Grade Count:5
Coefficient of Friction 1.30 - 2.731.30 - 2.73Average value: 1.69 Grade Count:4
Peel Strength 0.175 - 170 kN/m1.00 - 970 pliAverage value: 7.76 kN/m Grade Count:248
 0.1753 - 19.283 kN/m
@Temperature -55.0 - 177 °C
1.000 - 110.03 pli
@Temperature -67.0 - 351 °F
Average value: 4.83 kN/m Grade Count:26
 1.9283 - 4.5578 kN/m
@Temperature 65.6 - 121 °C
11.003 - 26.007 pli
@Temperature 150 - 250 °F
Average value: 4.83 kN/m Grade Count:3
 1.9283 - 4.5578 kN/m
@Time 1800 - 14400 sec
11.003 - 26.007 pli
@Time 0.500 - 4.00 hour
Average value: 4.83 kN/m Grade Count:3
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000100 - 5.00e+16 ohm-cm0.000100 - 5.00e+16 ohm-cmAverage value: 1.27e+15 ohm-cm Grade Count:486
 0.00200 - 6.00e+13 ohm-cm
@Temperature -3.89 - 260 °C
0.00200 - 6.00e+13 ohm-cm
@Temperature 25.0 - 500 °F
Average value: 9.96e+12 ohm-cm Grade Count:21
Surface Resistance 0.100 - 1.10e+17 ohm0.100 - 1.10e+17 ohmAverage value: 2.36e+16 ohm Grade Count:7
Dielectric Constant 2.70 - 67.52.70 - 67.5Average value: 5.49 Grade Count:369
 4.96 - 24.0
@Temperature 60.0 - 135 °C
4.96 - 24.0
@Temperature 140 - 275 °F
Average value: 5.32 Grade Count:6
 3.20 - 4.85
@Temperature 100 - 260 °C
3.20 - 4.85
@Temperature 212 - 500 °F
Average value: 5.32 Grade Count:10
 3.20 - 4.85
@Frequency 60.0 - 1.00e+6 Hz
3.20 - 4.85
@Frequency 60.0 - 1.00e+6 Hz
Average value: 5.32 Grade Count:10
Dielectric Strength 1.18 - 94.5 kV/mm30.0 - 2400 kV/inAverage value: 18.1 kV/mm Grade Count:305
Dissipation Factor 0.00200 - 0.3100.00200 - 0.310Average value: 0.0336 Grade Count:138
 0.0180 - 0.515
@Temperature 15.6 - 135 °C
0.0180 - 0.515
@Temperature 60.0 - 275 °F
Average value: 0.0784 Grade Count:6
 0.00300 - 0.422
@Temperature 60.0 - 260 °C
0.00300 - 0.422
@Temperature 140 - 500 °F
Average value: 0.0784 Grade Count:11
 0.00300 - 0.422
@Frequency 60.0 - 1.00e+6 Hz
0.00300 - 0.422
@Frequency 60.0 - 1.00e+6 Hz
Average value: 0.0784 Grade Count:11
Arc Resistance 26.0 - 130 sec26.0 - 130 secAverage value: 85.8 sec Grade Count:6
 
Thermal PropertiesMetricEnglishComments
CTE, linear 1.50 - 340 µm/m-°C0.833 - 189 µin/in-°FAverage value: 56.7 µm/m-°C Grade Count:419
 35.0 - 543 µm/m-°C
@Temperature -50.0 - 150 °C
19.4 - 302 µin/in-°F
@Temperature -58.0 - 302 °F
Average value: 159 µm/m-°C Grade Count:38
Specific Heat Capacity 0.300 J/g-°C0.0717 BTU/lb-°FAverage value: 0.300 J/g-°C Grade Count:3
Thermal Conductivity 0.100 - 41.8 W/m-K0.694 - 290 BTU-in/hr-ft²-°FAverage value: 1.87 W/m-K Grade Count:231
 0.147 - 0.184448 W/m-K
@Temperature 44.3 - 45.0 °C
1.02 - 1.28007 BTU-in/hr-ft²-°F
@Temperature 112 - 113 °F
Average value: 0.185 W/m-K Grade Count:9
 0.133 - 0.381 W/m-K
@Temperature 43.3 - 44.3 °C
0.923 - 2.64 BTU-in/hr-ft²-°F
@Temperature 110 - 112 °F
Average value: 0.185 W/m-K Grade Count:5
 0.133 - 0.381 W/m-K
@Thickness 6.35 - 6.35 mm
0.923 - 2.64 BTU-in/hr-ft²-°F
@Thickness 0.250 - 0.250 in
Average value: 0.185 W/m-K Grade Count:5
Maximum Service Temperature, Air 49.0 - 375 °C120 - 707 °FAverage value: 164 °C Grade Count:751
Deflection Temperature at 0.46 MPa (66 psi) 45.0 - 110 °C113 - 230 °FAverage value: 58.0 °C Grade Count:7
Deflection Temperature at 1.8 MPa (264 psi) 49.0 °C120 °FAverage value: 49.0 °C Grade Count:3
Heat Distortion Temperature 42.2 - 170 °C108 - 338 °FAverage value: 113 °C Grade Count:6
Minimum Service Temperature, Air -269 - -20.0 °C-453 - -4.00 °FAverage value: -73.4 °C Grade Count:621
Glass Transition Temp, Tg -50.0 - 300 °C-58.0 - 572 °FAverage value: 97.6 °C Grade Count:300
Decomposition Temperature 350 - 483 °C662 - 901 °FAverage value: 406 °C Grade Count:4
Flammability, UL94 HB - V-0HB - V-0Grade Count:5
Flash Point -14.0 - 205 °C6.80 - 401 °FAverage value: 99.8 °C Grade Count:42
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.50 - 1.631.50 - 1.63Average value: 1.55 Grade Count:65
Transmission, Visible 1.00 - 97.0 %1.00 - 97.0 %Average value: 86.9 % Grade Count:33
 
Processing PropertiesMetricEnglishComments
Processing Temperature 4.44 - 260 °C40.0 - 500 °FAverage value: 70.2 °C Grade Count:78
Cure Time 3.00 - 30200 min0.0500 - 504 hourAverage value: 2420 min Grade Count:488
 0.500 - 14400 min
@Temperature 30.0 - 250 °C
0.00833 - 240 hour
@Temperature 86.0 - 482 °F
Average value: 136 min Grade Count:625
 60.0 - 120 min
@Temperature 177 - 177 °C
1.00 - 2.00 hour
@Temperature 351 - 351 °F
Average value: 136 min Grade Count:3
 60.0 - 120 min
@Pressure 0.0689 - 0.0689 MPa
1.00 - 2.00 hour
@Pressure 10.0 - 10.0 psi
Average value: 136 min Grade Count:3
Tack-Free Time 9.00 - 540 min0.150 - 9.00 hourAverage value: 150 min Grade Count:12
Pot Life 0.500 - 389000 min0.500 - 389000 minAverage value: 2850 min Grade Count:619
 10.0 - 259200 min
@Temperature 10.0 - 40.0 °C
10.0 - 259200 min
@Temperature 50.0 - 104 °F
Average value: 104000 min Grade Count:5
 
Component Elements PropertiesMetricEnglishComments
Silver, Ag 65.0 - 75.0 %65.0 - 75.0 %Average value: 70.7 % Grade Count:3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Epoxy Adhesive, Flexible
Overview of materials for Epoxy/Carbon Fiber Composite
Overview of materials for Thermoset Polyurethane, Adhesive
Overview of materials for Epoxy Cure Resin
Overview of materials for Cyanoacrylate Adhesive

O1770 / 77902

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.