MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Aleris AA5024-H116 Aluminum Magnesium Scandium Alloy
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 5000 Series Aluminum Alloy

Material Notes: Features good weldability, excellent damage tolerance, good corrosion resistance, creep-formability. Aleris AlMgSc alloy AA5024 H116 allows simplification of the manufacturing process of aircraft fuselage components. With AA5024 H116 AlMgSc, stringer reinforced aircraft fuselage components can be either Laser Beam Welded (LBW) or Friction Stir Welded (FSW) when the individual parts are still flat, without any prior treatment. The single or double curvature of the fuselage part required for the aircraft body is achieved by creep forming at elevated temperature.

Recommended for use as fuselage skin sheet with medium strength but excellent damage tolerance and corrosion properties and can potentially replace traditionally used 2xxx alloys even as drop-in solution.

Temper, AMS and MMPDS registration pending. AA5024 H116 is covered by the Airbus specification AIMS 03-04-055

Information and property data for creep formed and welded (if applicable) sheet provided by Aleris.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.65 g/cc0.0957 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  315 MPa
@Thickness 1.60 mm
45700 psi
@Thickness 0.0630 in
LT Direction
 375 MPa
@Thickness 3.00 mm
54400 psi
@Thickness 0.118 in
LT Direction
 375 MPa
@Thickness 7.00 mm
54400 psi
@Thickness 0.276 in
LT Direction
 380 MPa
@Thickness 3.00 mm
55100 psi
@Thickness 0.118 in
L Direction
 380 MPa
@Thickness 7.00 mm
55100 psi
@Thickness 0.276 in
L Direction
 395 MPa
@Thickness 1.60 mm
57300 psi
@Thickness 0.0630 in
L Direction
Tensile Strength, Yield  305 MPa
@Thickness 3.00 mm
44200 psi
@Thickness 0.118 in
L Direction
 305 MPa
@Thickness 7.00 mm
44200 psi
@Thickness 0.276 in
L Direction
 305 MPa
@Thickness 3.00 mm
44200 psi
@Thickness 0.118 in
LT Direction
 305 MPa
@Thickness 7.00 mm
44200 psi
@Thickness 0.276 in
LT Direction
 310 MPa
@Thickness 1.60 mm
45000 psi
@Thickness 0.0630 in
LT Direction
 315 MPa
@Thickness 1.60 mm
45700 psi
@Thickness 0.0630 in
L Direction
Elongation at Break  15 %
@Thickness 1.60 mm
15 %
@Thickness 0.0630 in
L Direction
 15 %
@Thickness 3.00 mm
15 %
@Thickness 0.118 in
L Direction
 15 %
@Thickness 7.00 mm
15 %
@Thickness 0.276 in
L Direction
 17 %
@Thickness 7.00 mm
17 %
@Thickness 0.276 in
LT Direction
 18 %
@Thickness 3.00 mm
18 %
@Thickness 0.118 in
LT Direction
 19 %
@Thickness 1.60 mm
19 %
@Thickness 0.0630 in
LT Direction
Tensile Modulus 72.0 GPa10400 ksi
Compressive Strength  295 MPa
@Thickness 7.00 mm
42800 psi
@Thickness 0.276 in
L Direction
 300 MPa
@Thickness 7.00 mm
43500 psi
@Thickness 0.276 in
LT Direction
 305 MPa
@Thickness 3.00 mm
44200 psi
@Thickness 0.118 in
LT Direction
 305 MPa
@Thickness 3.00 mm
44200 psi
@Thickness 0.118 in
L Direction
 315 MPa
@Thickness 1.60 mm
45700 psi
@Thickness 0.0630 in
LT Direction
 325 MPa
@Thickness 1.60 mm
47100 psi
@Thickness 0.0630 in
L Direction
Compressive Modulus 74.0 GPa10700 ksi
Fatigue Strength  145 MPa
@# of Cycles 1.00e+6
21000 psi
@# of Cycles 1.00e+6
T-L
 145 MPa
@# of Cycles 300000
21000 psi
@# of Cycles 300000
T-L
 175 MPa
@# of Cycles 100000
25400 psi
@# of Cycles 100000
T-L
 180 MPa
@# of Cycles 80000
26100 psi
@# of Cycles 80000
T-L
 190 MPa
@# of Cycles 50000
27600 psi
@# of Cycles 50000
T-L
 290 MPa
@# of Cycles 10000
42100 psi
@# of Cycles 10000
T-L
 365 MPa
@# of Cycles 1000
52900 psi
@# of Cycles 1000
T-L
Fracture Toughness 35.0 MPa-m½31.9 ksi-in½Ke; T-L; Δae = 0 mm
 40.0 MPa-m½36.4 ksi-in½Ke; L-T; Δae = 0 mm
 90.0 MPa-m½81.9 ksi-in½Ke; T-L; Δae = 10 mm
 120 MPa-m½109 ksi-in½Ke; T-L; Δae = 20 mm
 120 MPa-m½109 ksi-in½Ke; L-T; Δae = 20 mm
 150 MPa-m½137 ksi-in½Ke; L-T; Δae = 40 mm
 155 MPa-m½141 ksi-in½Ke; T-L; Δae = 40 mm
 170 MPa-m½155 ksi-in½Ke; L-T; Δae = 60 mm
 175 MPa-m½159 ksi-in½Ke; T-L; Δae = 60 mm
 185 MPa-m½168 ksi-in½Ke; L-T; Δae = 80 mm
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 92.95 - 95.95 %92.95 - 95.95 %As Balance
Chromium, Cr <= 0.10 %<= 0.10 %
Copper, Cu <= 0.20 %<= 0.20 %
Iron, Fe <= 0.40 %<= 0.40 %
Magnesium, Mg 3.9 - 5.1 %3.9 - 5.1 %
Manganese, Mn <= 0.20 %<= 0.20 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Scandium, Sc 0.10 - 0.40 %0.10 - 0.40 %
Silicon, Si <= 0.25 %<= 0.25 %
Titanium, Ti <= 0.20 %<= 0.20 %
Zinc, Zn <= 0.25 %<= 0.25 %
Zirconium, Zr 0.05 - 0.20 %0.05 - 0.20 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 5024-H116 Al-Scandium Alloy
Aluminum 7075-T6; 7075-T651
5025 Aluminum Composition Spec
RSP Technology RSA-501 AE Aluminum Scandium Super Alloy (Scalmalloy)
Alclad Aluminum 7075-T6, T651

NALERIS88 / 161566

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.