MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ExxonMobil LLDPE LL 6101XR Wire & Cable Linear Low Density Polyethylene Resin (European Grade)
Categories: Polymer; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE)

Material Notes: Product Description: LL 6101 is a C4 Ziegler Natta LLDPE recommended for various compounding applications.

Availability: Africa & Middle East, Asia Pacific and Europe

Additive:

  • Antiblock: No
  • Thermal Stabilizer: Yes
Applications:
  • Cable compound applications
  • LV silane cross-linkable insulation – 1 step process
  • Masterbatch Base Resin

Information provided by ExxonMobil

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.924 g/cc0.0334 lb/in³ExxonMobil method
Melt Flow 20 g/10 min
@Load 2.16 kg,
Temperature 190 °C
20 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 7.00e+15 ohm-cm7.00e+15 ohm-cmASTM D257
Dielectric Constant 2.1
@Frequency 60 Hz
2.1
@Frequency 60 Hz
ASMT D150
Dielectric Strength 59.1 kV/mm1500 kV/in500 V/sec; ASTM D149
Dissipation Factor 0.00050
@Frequency 60 Hz
0.00050
@Frequency 60 Hz
ASMT D150
 
Thermal PropertiesMetricEnglishComments
Melting Point <= 123 °C<= 253 °FPeak Melting Point; ExxonMobil method

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ExxonMobil LLDPE LL 6100.17 Linear Low Density Polyethylene Resin
ExxonMobil LLDPE LL 5252.09 Linear Low Density Polyethylene Resin
ExxonMobil LLDPE LL 3404.48 Linear Low Density Polyethylene Resin
ExxonMobil LLDPE LL 3402.48 Blown Linear Low Density Polyethylene Resin
ExxonMobil LLDPE LL 1236.86 Linear Low Density Polyethylene Resin

PEX99191 / 175427

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.