MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Huntsman IROGRAN® A 85 E 5719 FCM TPU-Polyester
Categories: Polymer; Thermoplastic; Polyurethane, TP; Thermoplastic Polyurethane (TPUR), Polyester Grade

Material Notes: Introduction: IROGRAN A 85 E 5719 FCM is a thermoplastic polyester polyurethane for melt calendering. IROGRAN is part of the HUNTSMAN technical extrusion and injection molding product range and offers a specially designed, flexible material with a broad processing window. IROGRAN A 85 E 5719 FCM is a food contact material.

Performance Features:

  • High wear resistance
  • Good melt flow
  • High elasticity
  • Complies with FDA CFR 175.105 / 177.2600
Applications:
  • Textile Coatings
  • Technical molding
  • Cable jacketing

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.21 g/cc0.0437 lb/in³Injection molded parts; ASTM D792
Melt Index of Compound 60 g/10 min
@Load 10.0 kg,
Temperature 190 °C
60 g/10 min
@Load 22.0 lb,
Temperature 374 °F
MVR, [cm3/10 min]
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 8585Injection molded parts; ASTM D2240
Hardness, Shore D 3636Injection molded parts; ASTM D2240
Tensile Strength at Break 35.0 MPa5080 psiInjection molded parts; DIN 53504
Elongation at Break 620 %620 %Injection molded parts; DIN 53504
100% Modulus 6.00 MPa
@Strain 100 %
870 psi
@Strain 100 %
Injection molded parts; DIN 53504
300% Modulus 11.7 MPa
@Strain 300 %
1700 psi
@Strain 300 %
Injection molded parts; DIN 53504
Tear Strength 99.9 kN/m570 pliInjection molded parts; ASTM D624
Abrasion 2020mm3, Injection molded; DIN 53516
Compression Set  30 %
@Temperature 22.8 °C,
Time 86400 sec
30 %
@Temperature 73.0 °F,
Time 24.0 hour
Injection molded; ASTM D395
 42 %
@Temperature 70.0 °C,
Time 86400 sec
42 %
@Temperature 158 °F,
Time 24.0 hour
Injection molded; ASTM D395
 
Thermal PropertiesMetricEnglishComments
Melting Point 115 - 160 °C239 - 320 °F0.025" extruded film,
 
Processing PropertiesMetricEnglishComments
Feed Temperature 25.0 - 40.0 °C77.0 - 104 °FExtrusion
Middle Barrel Temperature 170 - 195 °C338 - 383 °FExtrusion
Nozzle Temperature 175 - 200 °C347 - 392 °FExtrusion
Adapter Temperature 175 - 200 °C347 - 392 °FExtrusion
Die Temperature 175 - 205 °C347 - 401 °FExtrusion
Roll Temperature 160 - 180 °C320 - 356 °FFront
 160 - 180 °C320 - 356 °FRear
 
Compliance PropertiesMetricEnglishComments
FDA YesYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Huntsman IROGRAN® A 60 E 4902 TPU-Polyester
Covestro DUREFLEX® U04 TPU
Huntsman IROGRAN® A 78 E 4723 Polyester-Based TPU-Injection Extrusion Grade
Huntsman IROGRAN® PS442-202 TPU-Polyester
Lubrizol Advanced Materials PEARLTHANE® Clear 15N85 Thermoplastic Polyurethane Elastomer

PHUQ095 / 159468

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.