MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Carpenter Pyromet® CTX-3 Superalloy, Heat Treated
Categories: Metal; Superalloy; Iron Base

Material Notes: Data provided by Carpenter Technology Corporation.

Pyromet® alloy CTX-3 is a high strength, precipitation hardenable superalloy which exhibits a low CTE over a broad temperature range. This alloy also possess high hot hardness and good thermal fatigue resistance. It is weldable, brazable, and can be chromium plated. This material offers significant improvement in notched stress-rupture strength over Pyromet alloy CTX-1. Retained hot-cold work is not required for good stress rupture properties and is not affected by stress orientation.

Pyromet® is a registered trademark of Carpenter Technology Corporation.

Key Words: Pyromet Alloy 907
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.28 g/cc0.299 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 1180 MPa171000 psi
 1040 MPa
@Temperature 538 °C
151000 psi
@Temperature 1000 °F
Tensile Strength, Yield 830 MPa
@Strain 0.2 %
120000 psi
@Strain 0.2 %
 673 MPa
@Strain 0.2 %,
Temperature 538 °C
97600 psi
@Strain 0.2 %,
Temperature 1000 °F
Elongation at Break 14 %14 %In 50 mm
 16 %
@Temperature 538 °C
16 %
@Temperature 1000 °F
In 50 mm
Reduction of Area 23 %23 %
 39 %
@Temperature 538 °C
39 %
@Temperature 1000 °F
Modulus of Elasticity 159.9 GPa23190 ksi
 
Thermal PropertiesMetricEnglishComments
CTE, linear  7.50 µm/m-°C
@Temperature 25.0 - 416 °C
4.17 µin/in-°F
@Temperature 77.0 - 781 °F
 7.70 µm/m-°C
@Temperature 25.0 - 260 °C
4.28 µin/in-°F
@Temperature 77.0 - 500 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al <= 0.25 %<= 0.25 %
Boron, B <= 0.012 %<= 0.012 %
Carbon, C <= 0.050 %<= 0.050 %
Chromium, Cr <= 0.50 %<= 0.50 %
Cobalt, Co 13 - 15 %13 - 15 %
Copper, Cu <= 0.50 %<= 0.50 %
Iron, Fe 39 %39 %as remainder
Manganese, Mn <= 0.50 %<= 0.50 %
Nb + Ta 4.5 - 5.5 %4.5 - 5.5 %
Nickel, Ni 37 - 39 %37 - 39 %
Niobium, Nb (Columbium, Cb) <= 5.5 %<= 5.5 %
Phosphorus, P <= 0.015 %<= 0.015 %
Silicon, Si <= 0.50 %<= 0.50 %
Sulfur, S <= 0.015 %<= 0.015 %
Tantalum, Ta <= 5.5 %<= 5.5 %
Titanium, Ti 1.25 - 1.75 %1.25 - 1.75 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
RSP Technology RSA-473 AH Aluminum Super Alloy
Carpenter Thermo-Span® Fe-Co-Ni Superalloy
Special Metals INCOLOY® Alloy 903
Special Metals INCOLOY® Alloy 907
Special Metals INCOLOY® Alloy 909

NCARD0 / 15747

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.