MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ovako 32CrMoV12-10* 398Q Steel, Hardening
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: General Information: Ovako 398Q is an ingot cast high tensile quench and tempering steel with high hardenability. The grade has high strength and toughness. The strong carbide and nitride formers makes it very well suited for nitriding. The grade is produced with the quality class IQ (isotropic quality). This ensures a very low number of elongated sulphide inclusions which will give more isotropic properties.

IQ-Steel(Isotropic Quality) is an isotropic quality ultra clean steel. IQ-Steel is optimized for fatigue strength by a strict control of steel cleanliness. IQ-Steel, a further development of BQ-Steel, is an isotropic and ultra clean steel with properties that match remelted steels. Based on thousands of examinations by Ovako into the effects of defects on fatigue performance, the metallurgy of IQ-Steel is purer and far more consistent than conventional grades, and designed specifically to perform well in multi axial loading. This enables the manufacturing of lighter, slimmed down components like gears, bearings and other critical parts. The steels are helping our customers to achieve new design solutions and implement higher standards of finished product performance. Key to these practical advantages are Ovako’s own unique, clean and consistent modern steelmaking processes that remove harmful inclusions and impurities from within the steel. IQ-Steels contain smaller and more fragmented inclusions and can handle much higher mechanical forces in all directions than conventional steels. IQ-Steels are newer, but already now well established in high pressure automotive applications. Modern diesel engines, with high and cyclic injection pressures, have proven to be an ideal application. Transmission components are another emerging area of strong interest.

Information provided by Ovako

Key Words: AMS 6481, W.Nr 1.7765
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 300300Tube, wall
Tensile Strength 940 MPa136000 psiTube, wall
Tensile Strength, Yield >= 800 MPa>= 116000 psiReh, Tube, wall
Elongation at Break 19 %19 %Tube, wall
Reduction of Area 70 %70 %Tube, wall
Modulus of Elasticity 210 GPa30500 ksi
Poissons Ratio 0.300.30
Shear Modulus 80.0 GPa11600 ksi
Impact Test  130 J
@Temperature 20.0 °C
95.9 ft-lb
@Temperature 68.0 °F
Tube, wall, transv
 200 J
@Temperature 20.0 °C
148 ft-lb
@Temperature 68.0 °F
Tube, wall, long
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000200 - 0.00000250 ohm-cm0.00000200 - 0.00000250 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 - 300 °C
6.67 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.460 - 0.480 J/g-°C
@Temperature 50.0 - 100 °C
0.110 - 0.115 BTU/lb-°F
@Temperature 122 - 212 °F
Thermal Conductivity 40.0 - 45.0 W/m-K278 - 312 BTU-in/hr-ft²-°FAmbient temperature
Transformation Temperature 357 °C675 °FMS
 773 °C1420 °FAC1
 884 °C1620 °FAC3
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.29 - 0.36 %0.29 - 0.36 %
Chromium, Cr 2.8 - 3.3 %2.8 - 3.3 %
Iron, Fe 93.37 - 95.56 %93.37 - 95.56 %As Balance
Manganese, Mn 0.40 - 0.70 %0.40 - 0.70 %
Molybdenum, Mo 0.70 - 1.2 %0.70 - 1.2 %
Nickel, Ni <= 0.30 %<= 0.30 %
Phosphorus, P <= 0.015 %<= 0.015 %
Silicon, Si 0.10 - 0.40 %0.10 - 0.40 %
Sulfur, S <= 0.0020 %<= 0.0020 %
Vanadium, V 0.15 - 0.35 %0.15 - 0.35 %
 
Descriptive Properties
WeldabilityCEV 1.48max
 Pcm 0.71max

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 6082-T6
ATI Allvac® 9310 UNS G93106, UNS H93100 Specialty Steel
Ovako 21CrMoV5-7 Imanite (6132) Steel, +QT
Ovako 40CrMoV4-6 6098 Steel, +QT
Ovako 34CrMo4 EN10083-3:2006 Steel

NOVAKO246 / 234545

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.