MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Total PPC 7652 Polypropylene, Heterophasic Copolymer, Injection Molding
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Molded

Material Notes: Polypropylene PPC 7652 is a nucleated and antistatic heterophasic copolymer with a Melt Flow index of 16 g/10 min.

Polypropylene PPC 7652 is a medium flow grade intended for a wide range of injection molding applications including battery cases, electrical appliance housings, toys, closures and lids.

Polypropylene PPC 7652 has been specially formulated to give antistatic performance.

Information provided by Total Petrochemicals.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.905 g/cc0.905 g/ccISO 1183
Bulk Density 0.525 g/cc0.0190 lb/in³ISO 1183
Melt Flow 16 g/10 min
@Load 2.16 kg,
Temperature 230 °C
16 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 8585ISO 2039-2
Tensile Strength, Yield 26.0 MPa3770 psiISO 527-2
Elongation at Yield 10 %10 %ISO 527-2
Tensile Modulus 1.45 GPa210 ksiISO 527-2
Flexural Modulus 1.35 GPa196 ksiISO 178
Izod Impact, Notched (ISO)  5.50 kJ/m²
@Temperature -20.0 °C
2.62 ft-lb/in²
@Temperature -4.00 °F
ISO 180
 9.00 kJ/m²
@Temperature 23.0 °C
4.28 ft-lb/in²
@Temperature 73.4 °F
ISO 180
Charpy Impact, Notched  0.600 J/cm²
@Temperature -20.0 °C
2.86 ft-lb/in²
@Temperature -4.00 °F
ISO 179
 1.00 J/cm²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
ISO 179
 
Thermal PropertiesMetricEnglishComments
Melting Point 165 °C329 °FISO 3146
Deflection Temperature at 0.46 MPa (66 psi) 92.0 °C198 °F120°C per hour; ISO 752
Deflection Temperature at 1.8 MPa (264 psi) 52.0 °C126 °F120°C per hour; ISO 752
Vicat Softening Point  75.0 °C
@Load 5.10 kg
167 °F
@Load 11.2 lb
50°C per hour; ISO 306
 145 °C
@Load 1.02 kg
293 °F
@Load 2.25 lb
50°C per hour; ISO 306

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
PolyMirae Moplen EP540R Injection Molding Grade Polypropylene
Total PPC 7650 Polypropylene, Heterophasic Copolymer

PTOTAL852 / 130577

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.