MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Mytex Polymers AS171L-02US Polypropylene, 13% Talc Filled
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 10% Talc Filler

Material Notes: AS171L-02US is a compounded thermoplastic polyolefin (TPO) designed for exterior automotive applications requiring cold temperature impact, processability and paintability.This product is available in natural or generic black. Applications: Exterior parts, Body Side Moldings, Claddings. OEM Approvals: Generam Motors GMW 15185, GMP.E/P.133

Data provided by Mytex Polymers

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.980 g/cc0.0354 lb/in³ISO 1183A
Linear Mold Shrinkage 0.0050 - 0.0070 cm/cm0.0050 - 0.0070 in/in48 hours after molding; ISO 294-3/4
 0.0060 - 0.0080 cm/cm
@Time 3600 sec
0.0060 - 0.0080 in/in
@Time 1.00 hour
48 hours after molding; ISO 294-3/4
 0.0070 - 0.0090 cm/cm
@Time 3600 sec
0.0070 - 0.0090 in/in
@Time 1.00 hour
48 hours after molding; ISO 294-3/4
Melt Flow 24 g/10 min
@Load 2.16 kg,
Temperature 230 °C
24 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133B
Ash 13 %
@Temperature 950 °C
13 %
@Temperature 1740 °F
ISO 3451/1A
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 15.0 MPa2180 psiISO 527-A/1A/50
Flexural Modulus 1.10 GPa160 ksi2 mm/min; ISO 178
Izod Impact, Notched (ISO) 54.0 kJ/m²
@Temperature 23.0 °C
25.7 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 50.0 °C122 °Funannealed; ISO 75-1/2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Global TPP-130 30% Talc Filled Polypropylene
Aclo Accutech Polypropylene CP0437T40V Copolymer Talc Reinforced
Asahi Kasei Thermylene® P-20TC-5100 20% Talc Filled, Heat Stabilized Polypropylene
Polyram RamOfin PPC359T4 Polypropylene, 20% Mineral Filled
Trinseo Magnum™ 347EZ ABS

PMYTEX031 / 99800

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.