MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Eastman D4032-F Polyethylene  (discontinued **)
Categories: Polymer; Thermoplastic; Polyethylene (PE); Low Density (LDPE)

Material Notes: D4032-F is a low density, fractional-melt formulation which contains no slip and medium antiblock. It is designed for film applications requiring exceptional toughness, such as in heavy-duty shipping sacks or in construction and agricultural films.

Information supplied by the manufacturer.

Information from manufacturer data sheet.

Eastman Chemical Company sold its polyethylene business to Westlake Chemical Corporation in Dec. 2006. This grade no longer appears in the Westlake product line.

Key Words: Exceptional toughness
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.921 g/cc0.0333 lb/in³ASTM D4883
Thickness 76.0 microns2.99 mil
Melt Flow 0.30 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.30 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 25.0 MPa3630 psiASTM D882
Film Tensile Strength at Yield, TD 11.0 MPa1600 psiASTM D882
Film Elongation at Break, MD 320 %320 %ASTM D882
Film Elongation at Break, TD 885 %885 %ASTM D882
Secant Modulus, MD 0.193 GPa28.0 ksi1% Secant; ASTM D882
Secant Modulus, TD 0.231 GPa33.5 ksi1% Secant; ASTM D882
Elmendorf Tear Strength MD 355 g355 g
Elmendorf Tear Strength TD 334 g334 g
Elmendorf Tear Strength, MD 4.66 g/micron118 g/milASTM D1922
Elmendorf Tear Strength, TD 4.33 g/micron110 g/milASTM D1922
Dart Drop 4.19 g/micron106 g/milASTM D1709A
Film Tensile Strength at Break, MD 23.0 MPa3340 psiASTM D882
Film Tensile Strength at Break, TD 23.0 MPa3340 psiASTM D882
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 95.0 °C203 °FASTM D1525
 
Optical PropertiesMetricEnglishComments
Haze 12 %12 %ASTM D1003
Gloss 53 %53 %at 45°; ASTM D2457
 
Descriptive Properties
ProcessFilm

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LyondellBasell Purell PE 1810E Low Density Polyethylene (LDPE)
Versalis Riblene® BD 30 Low Density Polyethylene - Blow Molding
Sibur 15303-003 Low Density Polyethylene
Chevron Phillips Marlex® 5628 LDPE Blown Film Resin
ExxonMobil LDPE LD 165BW1 Low Density Polyethylene Resin

PEAT360 / 35382

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.