MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

422 Stainless Steel, 455°C temper, short time elevated temperature test
Categories: Metal; Ferrous Metal; Stainless Steel; T 400 Series Stainless Steel

Material Notes: austenitized at 1040°C for 1 hour, oil quench, temper for 2 hours

Key Words: UNS S42200, AMS 5655, ASTM A565, SAE J467, DIN 1.4935, JIS SUH 616
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 1490 MPa
@Temperature 425 °C
216000 psi
@Temperature 797 °F
Tensile Strength, Yield 979 MPa
@Strain 0.2 %,
Temperature 425 °C
142000 psi
@Strain 0.2 %,
Temperature 797 °F
Elongation at Break 19 %
@Temperature 425 °C
19 %
@Temperature 797 °F
in 36 mm
Modulus of Elasticity 166.6 GPa
@Temperature 425 °C
24160 ksi
@Temperature 797 °F
Shear Modulus 72.4 GPa
@Temperature 425 °C
10500 ksi
@Temperature 797 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000610 ohm-cm0.0000610 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.2 µm/m-°C
@Temperature 0.000 - 100 °C
6.22 µin/in-°F
@Temperature 32.0 - 212 °F
 11.3 µm/m-°C
@Temperature 0.000 - 315 °C
6.28 µin/in-°F
@Temperature 32.0 - 599 °F
 11.9 µm/m-°C
@Temperature 0.000 - 540 °C
6.61 µin/in-°F
@Temperature 32.0 - 1000 °F
 12.1 µm/m-°C
@Temperature 0.000 - 650 °C
6.72 µin/in-°F
@Temperature 32.0 - 1200 °F
Specific Heat Capacity 0.460 J/g-°C
@Temperature 0.000 - 100 °C
0.110 BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity  23.9 W/m-K
@Temperature 100 °C
166 BTU-in/hr-ft²-°F
@Temperature 212 °F
 27.3 W/m-K
@Temperature 500 °C
189 BTU-in/hr-ft²-°F
@Temperature 932 °F
Melting Point 1470 - 1480 °C2680 - 2700 °F
Solidus 1470 °C2680 °F
Liquidus 1480 °C2700 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.20 - 0.25 %0.20 - 0.25 %
Chromium, Cr 12 %12 %
Iron, Fe 84 %84 %
Manganese, Mn <= 1.0 %<= 1.0 %
Molybdenum, Mo 1.0 %1.0 %
Nickel, Ni 0.75 %0.75 %
Phosphorus, P <= 0.025 %<= 0.025 %
Silicon, Si <= 0.75 %<= 0.75 %
Sulfur, S <= 0.025 %<= 0.025 %
Tungsten, W 1.0 %1.0 %
Vanadium, V 0.23 %0.23 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type 440B Stainless Steel
AK Steel 439 Ferritic Stainless steel
440A Martensitic Stainless Steel (UNS S44002)
416 Stainless Steel, annealed bar
422 Stainless Steel 315°C (600°F) temper

MQ422AC / 13086

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.