MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Lushan Solar EVA Film Lamination, Ultra Fast Cure
Categories: Polymer; Film; Thermoplastic; Ethylene Vinyl Acetate; Ethylene Vinyl Acetate Copolymer (EVA), Film Grade

Material Notes: EVA film for encapsulating solar module Lushan series with ultra fast cure characteristic is used as encapsulate materials for photovoltaic industry. With Innovative technology, Lushan ultra fast cure solar EVA film has developed to be a stable, high properties, and reputable products, and widely used in China and overseas market. Lushan ultra fast cure solar EVA film has very good processing properties that helps PV module manufactures with the most effective production way and save the cost as much as possible.

Information provided by Lushan

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Processing PropertiesMetricEnglishComments
Gel Time  0.000 min
@Temperature 135 °C
0.000 min
@Temperature 275 °F
0% Gel content
 0.000 min
@Temperature 138 °C
0.000 min
@Temperature 280 °F
0% Gel content
 0.000 min
@Temperature 140 °C
0.000 min
@Temperature 284 °F
0.02% Gel content
 0.000 min
@Temperature 143 °C
0.000 min
@Temperature 289 °F
0.09% Gel content
 0.000 min
@Temperature 145 °C
0.000 min
@Temperature 293 °F
0.21% Gel content
 0.000 min
@Temperature 148 °C
0.000 min
@Temperature 298 °F
1.6% Gel content
 0.000 min
@Temperature 150 °C
0.000 min
@Temperature 302 °F
3.59% Gel content
 0.000 min
@Temperature 153 °C
0.000 min
@Temperature 307 °F
42.8% Gel content
 0.000 min
@Temperature 155 °C
0.000 min
@Temperature 311 °F
61.11% Gel content
 3.00 min
@Temperature 135 °C
3.00 min
@Temperature 275 °F
0% Gel content
 3.00 min
@Temperature 138 °C
3.00 min
@Temperature 280 °F
23.17% Gel content
 3.00 min
@Temperature 140 °C
3.00 min
@Temperature 284 °F
25.7% Gel content
 3.00 min
@Temperature 143 °C
3.00 min
@Temperature 289 °F
53.3% Gel content
 3.00 min
@Temperature 145 °C
3.00 min
@Temperature 293 °F
43.5% Gel content
 3.00 min
@Temperature 148 °C
3.00 min
@Temperature 298 °F
71.81% Gel content
 3.00 min
@Temperature 150 °C
3.00 min
@Temperature 302 °F
79.16% Gel content
 3.00 min
@Temperature 153 °C
3.00 min
@Temperature 307 °F
80.27% Gel content
 3.00 min
@Temperature 155 °C
3.00 min
@Temperature 311 °F
83.62% Gel content
 5.00 min
@Temperature 135 °C
5.00 min
@Temperature 275 °F
3.39% Gel content
 5.00 min
@Temperature 138 °C
5.00 min
@Temperature 280 °F
46.51% Gel content
 5.00 min
@Temperature 140 °C
5.00 min
@Temperature 284 °F
53.77% Gel content
 5.00 min
@Temperature 143 °C
5.00 min
@Temperature 289 °F
71.9% Gel content
 5.00 min
@Temperature 145 °C
5.00 min
@Temperature 293 °F
70.85% Gel content
 5.00 min
@Temperature 148 °C
5.00 min
@Temperature 298 °F
81.33% Gel content
 5.00 min
@Temperature 150 °C
5.00 min
@Temperature 302 °F
84.59% Gel content
 5.00 min
@Temperature 153 °C
5.00 min
@Temperature 307 °F
85.91% Gel content
 5.00 min
@Temperature 155 °C
5.00 min
@Temperature 311 °F
88.68% Gel content
 8.00 min
@Temperature 135 °C
8.00 min
@Temperature 275 °F
50.98% Gel content
 8.00 min
@Temperature 138 °C
8.00 min
@Temperature 280 °F
64.91% Gel content
 8.00 min
@Temperature 140 °C
8.00 min
@Temperature 284 °F
75.72% Gel content
 8.00 min
@Temperature 143 °C
8.00 min
@Temperature 289 °F
82.31% Gel content
 8.00 min
@Temperature 145 °C
8.00 min
@Temperature 293 °F
85.12% Gel content
 8.00 min
@Temperature 148 °C
8.00 min
@Temperature 298 °F
87.17% Gel content
 8.00 min
@Temperature 150 °C
8.00 min
@Temperature 302 °F
89.42% Gel content
 8.00 min
@Temperature 153 °C
8.00 min
@Temperature 307 °F
88.74% Gel content
 8.00 min
@Temperature 155 °C
8.00 min
@Temperature 311 °F
89.18% Gel content
 10.0 min
@Temperature 150 °C
10.0 min
@Temperature 302 °F
89.38% Gel content
 10.0 min
@Temperature 153 °C
10.0 min
@Temperature 307 °F
90.26% Gel content
 10.0 min
@Temperature 155 °C
10.0 min
@Temperature 311 °F
89.93% Gel content
 10.0 min
@Temperature 135 °C
10.0 min
@Temperature 275 °F
66.37% Gel content
 10.0 min
@Temperature 138 °C
10.0 min
@Temperature 280 °F
77.72% Gel content
 10.0 min
@Temperature 140 °C
10.0 min
@Temperature 284 °F
81.8% Gel content
 10.0 min
@Temperature 143 °C
10.0 min
@Temperature 289 °F
84.41% Gel content
 10.0 min
@Temperature 145 °C
10.0 min
@Temperature 293 °F
87.77% Gel content
 10.0 min
@Temperature 148 °C
10.0 min
@Temperature 298 °F
88.48% Gel content
 13.0 min
@Temperature 135 °C
13.0 min
@Temperature 275 °F
75.71% Gel content
 13.0 min
@Temperature 138 °C
13.0 min
@Temperature 280 °F
79.7% Gel content
 13.0 min
@Temperature 140 °C
13.0 min
@Temperature 284 °F
84.53% Gel content
 13.0 min
@Temperature 143 °C
13.0 min
@Temperature 289 °F
86.24% Gel content
 13.0 min
@Temperature 145 °C
13.0 min
@Temperature 293 °F
86.85% Gel content
 13.0 min
@Temperature 148 °C
13.0 min
@Temperature 298 °F
88.92% Gel content
 13.0 min
@Temperature 150 °C
13.0 min
@Temperature 302 °F
88.91% Gel content
 13.0 min
@Temperature 153 °C
13.0 min
@Temperature 307 °F
89.95% Gel content
 13.0 min
@Temperature 155 °C
13.0 min
@Temperature 311 °F
89.9% Gel content
 15.0 min
@Temperature 135 °C
15.0 min
@Temperature 275 °F
79.98% Gel content
 15.0 min
@Temperature 138 °C
15.0 min
@Temperature 280 °F
83.72% Gel content
 15.0 min
@Temperature 140 °C
15.0 min
@Temperature 284 °F
86.78% Gel content
 15.0 min
@Temperature 143 °C
15.0 min
@Temperature 289 °F
87.12% Gel content
 15.0 min
@Temperature 145 °C
15.0 min
@Temperature 293 °F
89.11% Gel content
 15.0 min
@Temperature 148 °C
15.0 min
@Temperature 298 °F
89.94% Gel content
 15.0 min
@Temperature 150 °C
15.0 min
@Temperature 302 °F
89.6% Gel content
 15.0 min
@Temperature 153 °C
15.0 min
@Temperature 307 °F
89.41% Gel content
 15.0 min
@Temperature 155 °C
15.0 min
@Temperature 311 °F
90.16% Gel content
 18.0 min
@Temperature 135 °C
18.0 min
@Temperature 275 °F
82.27% Gel content
 18.0 min
@Temperature 138 °C
18.0 min
@Temperature 280 °F
85.13% Gel content
 18.0 min
@Temperature 140 °C
18.0 min
@Temperature 284 °F
86.94% Gel content
 18.0 min
@Temperature 143 °C
18.0 min
@Temperature 289 °F
89.65% Gel content
 18.0 min
@Temperature 145 °C
18.0 min
@Temperature 293 °F
88.31% Gel content
 18.0 min
@Temperature 148 °C
18.0 min
@Temperature 298 °F
90.91% Gel content
 18.0 min
@Temperature 150 °C
18.0 min
@Temperature 302 °F
90.45% Gel content
 18.0 min
@Temperature 153 °C
18.0 min
@Temperature 307 °F
89.27% Gel content
 18.0 min
@Temperature 155 °C
18.0 min
@Temperature 311 °F
90.77% Gel content
 20.0 min
@Temperature 150 °C
20.0 min
@Temperature 302 °F
89.8% Gel content
 20.0 min
@Temperature 153 °C
20.0 min
@Temperature 307 °F
90.39% Gel content
 20.0 min
@Temperature 155 °C
20.0 min
@Temperature 311 °F
90.35% Gel content
 20.0 min
@Temperature 135 °C
20.0 min
@Temperature 275 °F
82.76% Gel content
 20.0 min
@Temperature 138 °C
20.0 min
@Temperature 280 °F
85.82% Gel content
 20.0 min
@Temperature 140 °C
20.0 min
@Temperature 284 °F
87.83% Gel content
 20.0 min
@Temperature 143 °C
20.0 min
@Temperature 289 °F
88.2% Gel content
 20.0 min
@Temperature 145 °C
20.0 min
@Temperature 293 °F
89.31% Gel content
 20.0 min
@Temperature 148 °C
20.0 min
@Temperature 298 °F
89.14% Gel content

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Honeywell A-C® 405S EVA copolymer
ExxonMobil Escorene® LD 713.93 Cast Film Resin
Innospec FLEXAREN® 07002 EVA-Copolymer
Innospec FLEXAREN® 07000 EVA-Copolymer
ICO Polymers ICOTEX™ 520-5076 500 Micron EVA Powder

PLUSH009 / 150007

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.