MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

AGC AFLAS® 150P TFE/P Fluoroelastomers
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: Description: AFLAS® Fluoroelastomers are copolymers of tetrafluoroethylene and propylene. This combination gives AFLAS® Fluoroelastomers unique properties over conventional FKM-type fluoroelastomers in demanding applications found in the oil & gas, chemical process, wire & cable, industrial equipment, food handling, pharmaceutical, heavy duty diesel and automotive industries. AFLAS Fluoroelastomers display outstanding resistance to heat, acids & bases, many solvents, ozone, and steam. Classified by ASTM D 1418-01 as FEPM.

Material Features:

    Excellent base and amine resistance unmatched by FKM-type fluoroelastomers
  • Extremely high electrical resistivity, compared with other elastomers
  • High heat resistance compared to FKMs
  • Outstanding steam resistance
End User Benefits:
    Most versatile AFLAS grade
  • Good balance between properties and processability
  • Can be extruded into complex profiles
Typical Applications:
    O-rings
  • Gaskets
  • Seals
  • Hoses, tubes
  • Sheets

Information provided by AGC Chemicals Americas Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Mooney Viscosity  70
@Temperature 121 °C
70
@Temperature 250 °F
[kN/m], (ML1+10)
 95
@Temperature 100 °C
95
@Temperature 212 °F
[kN/m], (ML1+10)
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 17.0 MPa2470 psi
 14.79 MPa
@Treatment Temp. 175 °C,
Time 2.59e+6 sec
2145 psi
@Treatment Temp. 347 °F,
Time 720 hour
ASTM No.3 Oil Resistance
 15.47 MPa
@Treatment Temp. 175 °C,
Time 2.59e+6 sec
2244 psi
@Treatment Temp. 347 °F,
Time 720 hour
SM class Engine Oil Resistance
 15.64 MPa
@Treatment Temp. 180 °C,
Time 2.59e+6 sec
2268 psi
@Treatment Temp. 356 °F,
Time 720 hour
Steam Resistance
 17.34 MPa
@Treatment Temp. 200 °C,
Time 3.60e+6 sec
2515 psi
@Treatment Temp. 392 °F,
Time 1000 hour
Heat Resistance
 17.85 MPa
@Treatment Temp. 70.0 °C,
Time 2.59e+6 sec
2589 psi
@Treatment Temp. 158 °F,
Time 720 hour
50% NaOH aq Resistance
Elongation at Break 280 %280 %
 257.6 %
@Treatment Temp. 175 °C,
Time 2.59e+6 sec
257.6 %
@Treatment Temp. 347 °F,
Time 720 hour
SM class Engine Oil Resistance
 260.4 %
@Treatment Temp. 200 °C,
Time 3.60e+6 sec
260.4 %
@Treatment Temp. 392 °F,
Time 1000 hour
Heat Resistance
 266 %
@Treatment Temp. 175 °C,
Time 2.59e+6 sec
266 %
@Treatment Temp. 347 °F,
Time 720 hour
ASTM No.3 Oil Resistance
 294 %
@Treatment Temp. 70.0 °C,
Time 2.59e+6 sec
294 %
@Treatment Temp. 158 °F,
Time 720 hour
50% NaOH aq Resistance
 310.8 %
@Treatment Temp. 180 °C,
Time 2.59e+6 sec
310.8 %
@Treatment Temp. 356 °F,
Time 720 hour
Steam Resistance
Tensile Modulus 0.000240 GPa0.0348 ksiG' Storage Modulus (nominal) of Raw Gum
100% Modulus 5.00 MPa
@Strain 100 %
725 psi
@Strain 100 %
Compression Set 29 %
@Temperature 200 °C,
Time 252000 sec
29 %
@Temperature 392 °F,
Time 70.0 hour
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -40.0 °C-40.0 °FBrittle Point
 3.00 °C37.4 °FTR-10
Glass Transition Temp, Tg -3.00 °C26.6 °F
 
Processing PropertiesMetricEnglishComments
Cure Time  1.90 min
@Temperature 177 °C
0.0317 hour
@Temperature 351 °F
50% cure, tc50, 100CPM, 3° Strain, 12 minutes
 6.50 min
@Temperature 177 °C
0.108 hour
@Temperature 351 °F
90% cure, 100CPM, 3° Strain, 12 minutes
 20.0 min
@Temperature 170 °C
0.333 hour
@Temperature 338 °F
Press
 240 min
@Temperature 200 °C
4.00 hour
@Temperature 392 °F
Post cure
 
Component Elements PropertiesMetricEnglishComments
Fluorine, F 57 %57 %
 
Descriptive Properties
Cure Data41.3 dNmMax S'
 6.0 dNmMin S'
Volume Change0%50% NaOH Resistance 70°C for 720 hours
Volume Change (%)15ASTM No.3 Oil Resistance 175°C for 720 hours
 7SM class Engine Oil Resistance 175°C for 720 hours

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AGC AFLAS® PM-1100 TFE/P Perfluoroelastomer
AGC AFLAS® 150C TFE/P Fluoroelastomers
AGC AFLAS® 300S TFE/P Latex
AGC AFLAS® 200P TFE/P Fluoroelastomers
AGC AFLAS® 150L TFE/P Fluoroelastomers

PAGCX009 / 191118

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.