MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Toyobo PELPRENE™ P90B Polyester TPE
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyester TPE; Polyester, TP; Polyester Thermoplastic Elastomer

Material Notes: Features: Polyester TPE

Information provided by Toyobo.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.19 g/cc0.0430 lb/in³ASTM D792
Moisture Absorption at Equilibrium 0.40 %0.40 %23°C, 65% RH
Linear Mold Shrinkage 0.011 cm/cm
@Thickness 2.00 mm
0.011 in/in
@Thickness 0.0787 in
Melt Index of Compound 20 g/10 min
@Temperature 230 °C
20 g/10 min
@Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 9696JIS K6301
Hardness, Shore D 5252ASTM D2240
Tensile Strength at Break 31.0 MPa4500 psiASTM D638
Elongation at Break 700 %700 %ASTM D638
50% Modulus 14.7 MPa
@Strain 50 %
14.7 MPa
@Strain 50 %
ASTM D638
Flexural Modulus 0.162 GPa23.5 ksiASTM D790
Compressive Modulus 0.0133 GPa1.93 ksi10%; ASTM D695
Resilience 6565JIS K6301
Izod Impact, Notched NBNBASTM D256
Tear Strength 172 kN/m981 pliASTM D624
Taber Abrasion, mg/1000 Cycles 1313ASTM D1044
Compression Set 57 %57 %JIS K6301
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 6.00e+13 ohm-cm6.00e+13 ohm-cmASTM D257
Dielectric Strength 30.0 kV/mm762 kV/inJIS K2111
 
Thermal PropertiesMetricEnglishComments
CTE, linear 140 µm/m-°C
@Temperature 20.0 °C
77.8 µin/in-°F
@Temperature 68.0 °F
TMA
Melting Point 203 °C397 °FBy DSC
Maximum Service Temperature, Air 101 °C214 °FHeat deflection temperature, load unknown; ASTM D648
Vicat Softening Point 180 °C356 °FASTM D1525
Brittleness Temperature <= -65.0 °C<= -85.0 °FJIS K6301
Flammability, UL94 HBHB

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Riteflex® 647 Thermoplastic Polyester Elastomer (TPE)
Envalior Arnitel® EL550 Polyether Ester Elastomer (European and Asian Grade)
Toyobo PELPRENE™ P55B Polyester TPE
Celanese Riteflex® 635 Thermoplastic Polyester Elastomer (TPE)
Eastman Neostar FN005 Elastomer

PTOY668 / 70828

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.