Physical Properties | Metric | English | Comments |
---|
Density | 9.22 g/cc | 0.333 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 434 | 434 |
Hardness, Knoop | 478 | 478 |
Hardness, Rockwell C | 46 | 46 |
Hardness, Vickers | 459 | 459 |
Tensile Strength, Ultimate | 1525 MPa | 221200 psi |
Tensile Strength, Yield | 1260 MPa @Strain 0.2 % | 183000 psi @Strain 0.2 % |
Elongation at Break | 8.0 % | 8.0 % |
Modulus of Elasticity | 216 GPa | 31300 ksi |
| 147 GPa @Temperature 1000 °C | 21300 ksi @Temperature 1830 °F |
| 157 GPa @Temperature 900 °C | 22800 ksi @Temperature 1650 °F |
| 168 GPa @Temperature 800 °C | 24400 ksi @Temperature 1470 °F |
| 178 GPa @Temperature 700 °C | 25800 ksi @Temperature 1290 °F |
| 185 GPa @Temperature 600 °C | 26800 ksi @Temperature 1110 °F |
| 190 GPa @Temperature 500 °C | 27600 ksi @Temperature 932 °F |
| 197 GPa @Temperature 400 °C | 28600 ksi @Temperature 752 °F |
| 202 GPa @Temperature 300 °C | 29300 ksi @Temperature 572 °F |
| 208 GPa @Temperature 200 °C | 30200 ksi @Temperature 392 °F |
| 213 GPa @Temperature 100 °C | 30900 ksi @Temperature 212 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.000137 ohm-cm | 0.000137 ohm-cm |
| 0.000130 ohm-cm @Temperature 1000 °C | 0.000130 ohm-cm @Temperature 1830 °F |
| 0.000132 ohm-cm @Temperature 900 °C | 0.000132 ohm-cm @Temperature 1650 °F |
| 0.000137 ohm-cm @Temperature 800 °C | 0.000137 ohm-cm @Temperature 1470 °F |
| 0.000137 ohm-cm @Temperature 100 °C | 0.000137 ohm-cm @Temperature 212 °F |
| 0.000137 ohm-cm @Temperature 200 °C | 0.000137 ohm-cm @Temperature 392 °F |
| 0.000138 ohm-cm @Temperature 300 °C | 0.000138 ohm-cm @Temperature 572 °F |
| 0.000138 ohm-cm @Temperature 400 °C | 0.000138 ohm-cm @Temperature 752 °F |
| 0.000140 ohm-cm @Temperature 500 °C | 0.000140 ohm-cm @Temperature 932 °F |
| 0.000142 ohm-cm @Temperature 700 °C | 0.000142 ohm-cm @Temperature 1290 °F |
| 0.000143 ohm-cm @Temperature 600 °C | 0.000143 ohm-cm @Temperature 1110 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 11.4 µm/m-°C @Temperature 25.0 - 300 °C | 6.33 µin/in-°F @Temperature 77.0 - 572 °F |
| 11.6 µm/m-°C @Temperature 25.0 - 400 °C | 6.44 µin/in-°F @Temperature 77.0 - 752 °F |
| 11.8 µm/m-°C @Temperature 25.0 - 600 °C | 6.56 µin/in-°F @Temperature 77.0 - 1110 °F |
| 11.8 µm/m-°C @Temperature 25.0 - 500 °C | 6.56 µin/in-°F @Temperature 77.0 - 932 °F |
| 12.2 µm/m-°C @Temperature 25.0 - 700 °C | 6.78 µin/in-°F @Temperature 77.0 - 1290 °F |
| 13.1 µm/m-°C @Temperature 25.0 - 800 °C | 7.28 µin/in-°F @Temperature 77.0 - 1470 °F |
| 13.9 µm/m-°C @Temperature 25.0 - 900 °C | 7.72 µin/in-°F @Temperature 77.0 - 1650 °F |
| 14.4 µm/m-°C @Temperature 25.0 - 1000 °C | 8.00 µin/in-°F @Temperature 77.0 - 1830 °F |
Specific Heat Capacity | 0.373 J/g-°C | 0.0891 BTU/lb-°F |
| 0.382 J/g-°C @Temperature 100 °C | 0.0913 BTU/lb-°F @Temperature 212 °F |
| 0.409 J/g-°C @Temperature 200 °C | 0.0978 BTU/lb-°F @Temperature 392 °F |
| 0.421 J/g-°C @Temperature 300 °C | 0.101 BTU/lb-°F @Temperature 572 °F |
| 0.431 J/g-°C @Temperature 400 °C | 0.103 BTU/lb-°F @Temperature 752 °F |
| 0.434 J/g-°C @Temperature 600 °C | 0.104 BTU/lb-°F @Temperature 1110 °F |
| 0.436 J/g-°C @Temperature 500 °C | 0.104 BTU/lb-°F @Temperature 932 °F |
| 0.575 J/g-°C @Temperature 1000 °C | 0.137 BTU/lb-°F @Temperature 1830 °F |
| 0.577 J/g-°C @Temperature 900 °C | 0.138 BTU/lb-°F @Temperature 1650 °F |
| 0.589 J/g-°C @Temperature 800 °C | 0.141 BTU/lb-°F @Temperature 1470 °F |
| 0.595 J/g-°C @Temperature 700 °C | 0.142 BTU/lb-°F @Temperature 1290 °F |
Thermal Conductivity | 11.2 W/m-K | 77.7 BTU-in/hr-ft²-°F |
| 12.1 W/m-K @Temperature 100 °C | 84.0 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 13.4 W/m-K @Temperature 200 °C | 93.0 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 14.8 W/m-K @Temperature 300 °C | 103 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 16.3 W/m-K @Temperature 400 °C | 113 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 17.9 W/m-K @Temperature 500 °C | 124 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 19.6 W/m-K @Temperature 600 °C | 136 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 21.4 W/m-K @Temperature 700 °C | 149 BTU-in/hr-ft²-°F @Temperature 1290 °F |
| 21.4 W/m-K @Temperature 800 °C | 149 BTU-in/hr-ft²-°F @Temperature 1470 °F |
| 23.3 W/m-K @Temperature 900 °C | 162 BTU-in/hr-ft²-°F @Temperature 1650 °F |
| 27.5 W/m-K @Temperature 1000 °C | 191 BTU-in/hr-ft²-°F @Temperature 1830 °F |
Melting Point | 1370 - 1418 °C | 2500 - 2584 °F |
Solidus | 1370 °C | 2500 °F |
Liquidus | 1418 °C | 2584 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Aluminum, Al | <= 0.50 % | <= 0.50 % |
Carbon, C | <= 0.010 % | <= 0.010 % |
Chromium, Cr | 1.5 % | 1.5 % |
Cobalt, Co | <= 3.0 % | <= 3.0 % |
Iron, Fe | 1.5 % | 1.5 % |
Manganese, Mn | <= 3.0 % | <= 3.0 % |
Molybdenum, Mo | 28.5 % | 28.5 % |
Nickel, Ni | >= 65 % | >= 65 % |
Silicon, Si | <= 0.10 % | <= 0.10 % |
Titanium, Ti | <= 0.20 % | <= 0.20 % |
Tungsten, W | <= 3.0 % | <= 3.0 % |
|
Descriptive Properties |
---|
Thermal Diffusivity | 0.003 cm2/s |
| 0.0032 cm2/s |
| 0.0034 cm2/s |
| 0.0037 cm2/s |
| 0.004 cm2/s |
| 0.0044 cm2/s |
| 0.0045 cm2/s |
| 0.0045 cm2/s |
| 0.0047 cm2/s |
| 0.0049 cm2/s |
| 0.0049 cm2/s |