MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Isoflon PEHD 300 High Density Polyethylene
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE)

Material Notes:
  • Products with excellent friction, anti-stick, abrasion and chemical inertia characteristics
  • Very good impact resistance
  • No moisture regain
  • Product for the food industry

Information provided by Isoflon.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.950 g/cc0.950 g/ccDIN 53479
Water Absorption 0.00 %0.00 %ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6363DIN 53505
Tensile Strength 24.0 MPa3480 psiDIN 53455
Elongation at Break 800 %800 %DIN 53455
Tensile Modulus 0.750 GPa109 ksiDIN 53457
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+17 ohm-cm1.00e+17 ohm-cmDIN 53482
Dielectric Constant 2.4
@Frequency 1000 Hz
2.4
@Frequency 1000 Hz
DIN 53483
Dielectric Strength 50.0 - 90.0 kV/mm1270 - 2290 kV/inDIN 53481
 
Thermal PropertiesMetricEnglishComments
CTE, linear 200 µm/m-°C111 µin/in-°FDIN 52328
Thermal Conductivity 0.430 W/m-K2.98 BTU-in/hr-ft²-°FDIN 52612
Melting Point 127 °C261 °FDIN 53736
Maximum Service Temperature, Air 80.0 °C176 °FContinuous; DIN 52612
Deflection Temperature at 1.8 MPa (264 psi) 55.0 °C131 °F
Minimum Service Temperature, Air -50.0 °C-58.0 °FContinuous; DIN 52612
Flammability, UL94 HBHB
 
Descriptive Properties
ColorNat./Black

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Isoflon PEHD 1000 High Density Polyethylene
Isoflon PEHD 500 High Density Polyethylene
Entec Hypel® PEHD.3/.955 HDPE
Mitsubishi Chemical Advanced Materials TIVAR™ UV UHMW-PE, Natural & Colored Except Black
Celanese Celstran® PEHD-GF40-01 PE-HD, 40% Glass Reinforced

PISOFL922 / 123310

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.