MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ExxonMobil Santoprene® 121-80B230 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: A soft, black thermoplastic vulcanizate (TPV) in the thermoplastic elastomer (TPE) family. This material is specially formulated to bond to sulfur or peroxide-cured thermoset EPDM rubber for corner molding, end caps and special fixation applications, and for COF enhancement. This grade of Santoprene TPV is shear-dependent and can be processed on conventional thermoplastics equipment for injection molding. It is polyolefin based and completely recyclable.

Key Benefits:

  • Specially formulated to replace thermoset EPDM rubber in automotive glass run channel corner molding applications.
  • Designed for shorter processing time compared to thermoset EPDM rubber.
  • Adheres to vulcanized EPDM rubber over wide range of temperatures.
  • Adheres to TPV over wide range of temperatures.
  • Enhanced COF properties.
  • EU and China RoHS compliant.
Applications:
  • Automotive- Weather Seals
Uses:
  • Automotive Applications
  • Automotive Exterior Trim
Availability: Africa & Middle East, Europe, North America, Asia Pacific, Latin America and South America

Information provided by Advanced Elastomer Systems

Key Words: EU 2003/11/EC; RoHS Compliant
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.920 g/cc0.920 g/ccASTM D792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 79792 mm, 15 sec; ISO 868
Tensile Strength at Break 8.27 MPa1200 psiAcross Flow; ASTM D412
Tensile Stress at Strain 3.30 MPa
@Strain 100 %
479 psi
@Strain 100 %
Across Flow; ASTM D412
Elongation at Break 500 %500 %Across Flow; ASTM D412
Compression Set 50 %
@Temperature 53.3 °C,
Time 79200 sec
50 %
@Temperature 128 °F,
Time 22.0 hour
ASTM D395
 
Processing PropertiesMetricEnglishComments
Processing Temperature 175 - 230 °C347 - 446 °F
 
Descriptive Properties
ColorBlack
FormPellets

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ExxonMobil Santoprene® 121-79W233 Thermoplastic Elastomer
ExxonMobil Santoprene® 121-70B230 Thermoplastic Elastomer
ExxonMobil Santoprene® 521-70 Thermoplastic Rubber
ExxonMobil Santoprene® 121-65W233 Thermoplastic Elastomer
ExxonMobil Santoprene® 121-80 Thermoplastic Elastomer

PADVA070 / 22760

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.