MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Röchling Formaterm® PC/ABS professional
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced

Material Notes: Product characteristics:
  • Good vacuum forming properties
  • High breaking strength and extremely high impact strength
  • High temperature resistance
Product applications:
  • Vacuum forming industry
  • Sports and leisure industry
  • Vehicle construction

Information provided by Röchling.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.19 g/cc0.0430 lb/in³DIN EN ISO 1183-1
Water Absorption 0.40 - 0.60 %0.40 - 0.60 %DIN EN ISO 62
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8585DIN EN ISO 868
Tensile Strength, Yield 69.0 MPa10000 psiDIN EN ISO 527
Elongation at Break 50 %50 %DIN EN ISO 527
Modulus of Elasticity 2.75 GPa399 ksiDIN EN ISO 527
Izod Impact, Notched (ISO) 45.0 kJ/m²21.4 ft-lb/in²DIN EN ISO 179
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+16 ohm-cm>= 1.00e+16 ohm-cmDIN EN 62631-3-1
Surface Resistance >= 1.00e+14 ohm>= 1.00e+14 ohmDIN EN 62631-3-2
Dielectric Constant 3.43.4IEC 60250
Dielectric Strength 20.0 kV/mm508 kV/inIEC 60243
Dissipation Factor 0.0080
@Frequency 1e+6 Hz
0.0080
@Frequency 1e+6 Hz
IEC 60250
 
Thermal PropertiesMetricEnglishComments
CTE, linear 60.0 - 110 µm/m-°C33.3 - 61.1 µin/in-°FDIN 53752
Thermal Conductivity 0.200 W/m-K1.39 BTU-in/hr-ft²-°FDIN 52612-1
Maximum Service Temperature, Air 105 °C221 °Fshort term
 110 °C230 °Flong term
Vicat Softening Point 113 °C235 °FDIN EN ISO 306, Vicat B
Minimum Service Temperature, Air -50.0 °C-58.0 °F
Glass Transition Temp, Tg 120 °C248 °FISO 11357-3
Flammability, UL94  V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
 V-0
@Thickness 6.00 mm
V-0
@Thickness 0.236 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Trinseo EMERGE™ PC/ABS 7700 NA Polycarbonate Resin
RTP Company RTP 2599 X 67122 Polycarbonate/ABS Alloy (PC/ABS), Unreinforced - Flame Retardant - Halogen Free - UL94 V-0
RTP Company RTP 2500 A Polycarbonate/ABS Alloy (PC/ABS)
Covestro Bayblend® FR 3010 Polycarbonate + ABS, Flame Retardant Grade
Mitsubishi Iupilon® MB 2213R PC/ABS

PROCH9156 / 232859

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.