MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Solvay CYCOM® 977-3 Epoxy - Unidirectional Carbon Fiber Tape
Categories: Polymer; Thermoset; Carbon Fiber/Thermoset Composite; Epoxy; Epoxy/Carbon Fiber Composite

Material Notes: CYCOM® 977-3 is a 350°F (177°C) curing resin. It is a toughened epoxy resin with 350°F (177°C) dry and 270°F (132°C) wet service capability. CYCOM 977-3 is formulated for autoclave or press molding and can be cured at 350°F (177°C) for six hours. Unidirectional tape and woven fabric impregnated with CYCOM 977-3 resin will retain tack for 21 days at 72°F (22°C). It has a long mechanical out life suitable for fabrication of large structures.

Features & Benefits:

  • 350°F (177°C) cure
  • Available on fabric and tape
  • 350°F (177°C) dry service temperature
  • 270°F (132°C) wet service temperature
  • Laminate and sandwich panel usage
  • Autoclave or press mold processing
  • Toughened epoxy using proprietary “cocontinuous”morphology
  • Impact resistance
  • Shelf life of 12 months at 0°F (-18°C), 21 days at 72°F (22°C)
Applications:
  • Aircraft primary and secondary structure
  • Applications where impact resistance is critical
  • Applications where hot/wet performance is crucial
Mechanical property data for 977-3 epoxy Unidirectional Tape with IM7 12K Intermediate Modulus Carbon Fiber [40 msi (276 GPa)].

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 2.51 MPa
@Temperature 24.0 °C
364 psi
@Temperature 75.2 °F
Elongation at Break 1.46 %1.46 %
Tensile Modulus 162 GPa
@Temperature 24.0 °C
23500 ksi
@Temperature 75.2 °F
Flexural Strength  1120 MPa
@Temperature 121 °C
162000 psi
@Temperature 250 °F
0°, wet
 1770 MPa
@Temperature 24.0 °C
256000 psi
@Temperature 75.2 °F
Flexural Modulus  146 GPa
@Temperature 121 °C
21200 ksi
@Temperature 250 °F
0°, wet
 150 GPa
@Temperature 24.0 °C
21800 ksi
@Temperature 75.2 °F
0°, Note 2
Compressive Strength  193.1 MPa
@Temperature 24.0 °C
28010 psi
@Temperature 75.2 °F
After 270 in-lb Impact
 1344 MPa
@Temperature 121 °C
194900 psi
@Temperature 250 °F
0°, wet
 1682 MPa
@Temperature 24.0 °C
244000 psi
@Temperature 75.2 °F
RDS, 10°C/minute)
Compressive Modulus  146 GPa
@Temperature 121 °C
21200 ksi
@Temperature 250 °F
0°, wet
 154 GPa
@Temperature 24.0 °C
22300 ksi
@Temperature 75.2 °F
Shear Strength  78.6 MPa
@Temperature 121 °C
11400 psi
@Temperature 250 °F
0° Interlaminar, wet
 128 MPa
@Temperature 24.0 °C
18500 psi
@Temperature 75.2 °F
0° Interlaminar
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 132 °C270 °Fwet
 177 °C351 °Fdry
Glass Transition Temp, Tg 178 °C352 °FG'
 189 °C372 °FG"
 190 °C374 °FTan Delta
 
Processing PropertiesMetricEnglishComments
Processing Temperature 177 °C350 °FCure
Shelf Life  0.630 Month
@Temperature 22.2 °C
0.630 Month
@Temperature 72.0 °F
 12.0 Month
@Temperature -17.8 °C
12.0 Month
@Temperature 0.000 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Solvay CYCOM® 5250-4 RTM BMI Resin, Composite with IM7-6K-4HS Fabric
Solvay CYCOM® 5250-4 RTM BMI Resin, Composite with T650-35-3K-PW Fabric
Solvay CYCOM® 5320-1 Epoxy with T40/800B Unidirectional Tape Composite
Solvay CYCOM® 890 RTM Resin - Woven Carbon Fabric Composite
Solvay CYCOM® 977-2 Epoxy - Carbon Fiber Laminate

PCYTED091b / 234747

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.