Physical Properties | Metric | English | Comments |
---|
Density | 8.64 g/cc | 0.312 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength, Ultimate | 784 MPa | 114000 psi |
Tensile Strength, Yield | 429 MPa @Strain 0.2 % | 62200 psi @Strain 0.2 % |
Elongation at Break | 48 % | 48 % |
Modulus of Elasticity | 211 GPa | 30600 ksi |
| 141 GPa @Temperature 982 °C | 20500 ksi @Temperature 1800 °F |
| 152 GPa @Temperature 871 °C | 22000 ksi @Temperature 1600 °F |
| 162 GPa @Temperature 760 °C | 23500 ksi @Temperature 1400 °F |
| 171 GPa @Temperature 649 °C | 24800 ksi @Temperature 1200 °F |
| 179 GPa @Temperature 538 °C | 26000 ksi @Temperature 1000 °F |
| 187 GPa @Temperature 427 °C | 27100 ksi @Temperature 801 °F |
| 194 GPa @Temperature 316 °C | 28100 ksi @Temperature 601 °F |
| 201 GPa @Temperature 204 °C | 29200 ksi @Temperature 399 °F |
| 207 GPa @Temperature 93.0 °C | 30000 ksi @Temperature 199 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.000125 ohm-cm @Temperature 23.0 °C | 0.000125 ohm-cm @Temperature 73.4 °F |
| 0.000125 ohm-cm @Temperature 100 °C | 0.000125 ohm-cm @Temperature 212 °F |
| 0.000126 ohm-cm @Temperature 200 °C | 0.000126 ohm-cm @Temperature 392 °F |
| 0.000127 ohm-cm @Temperature 300 °C | 0.000127 ohm-cm @Temperature 572 °F |
| 0.000128 ohm-cm @Temperature 400 °C | 0.000128 ohm-cm @Temperature 752 °F |
| 0.000129 ohm-cm @Temperature 500 °C | 0.000129 ohm-cm @Temperature 932 °F |
| 0.000132 ohm-cm @Temperature 600 °C | 0.000132 ohm-cm @Temperature 1110 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 10.8 µm/m-°C @Temperature 20.0 - 93.0 °C | 6.00 µin/in-°F @Temperature 68.0 - 199 °F |
| 11.9 µm/m-°C @Temperature 20.0 - 204 °C | 6.61 µin/in-°F @Temperature 68.0 - 399 °F |
| 12.6 µm/m-°C @Temperature 20.0 - 316 °C | 7.00 µin/in-°F @Temperature 68.0 - 601 °F |
| 13.3 µm/m-°C @Temperature 20.0 - 427 °C | 7.39 µin/in-°F @Temperature 68.0 - 801 °F |
| 13.3 µm/m-°C @Temperature 20.0 - 538 °C | 7.39 µin/in-°F @Temperature 68.0 - 1000 °F |
| 13.5 µm/m-°C @Temperature 20.0 - 649 °C | 7.50 µin/in-°F @Temperature 68.0 - 1200 °F |
| 14.4 µm/m-°C @Temperature 20.0 - 760 °C | 8.00 µin/in-°F @Temperature 68.0 - 1400 °F |
| 14.9 µm/m-°C @Temperature 24.0 - 871 °C | 8.28 µin/in-°F @Temperature 75.2 - 1600 °F |
| 15.7 µm/m-°C @Temperature 20.0 - 982 °C | 8.72 µin/in-°F @Temperature 68.0 - 1800 °F |
Specific Heat Capacity | 0.406 J/g-°C @Temperature 0.000 °C | 0.0970 BTU/lb-°F @Temperature 32.0 °F |
| 0.427 J/g-°C @Temperature 100 °C | 0.102 BTU/lb-°F @Temperature 212 °F |
| 0.448 J/g-°C @Temperature 200 °C | 0.107 BTU/lb-°F @Temperature 392 °F |
| 0.465 J/g-°C @Temperature 300 °C | 0.111 BTU/lb-°F @Temperature 572 °F |
| 0.477 J/g-°C @Temperature 400 °C | 0.114 BTU/lb-°F @Temperature 752 °F |
| 0.490 J/g-°C @Temperature 500 °C | 0.117 BTU/lb-°F @Temperature 932 °F |
| 0.502 J/g-°C @Temperature 600 °C | 0.120 BTU/lb-°F @Temperature 1110 °F |
Thermal Conductivity | 10.1 W/m-K @Temperature 23.0 °C | 70.1 BTU-in/hr-ft²-°F @Temperature 73.4 °F |
| 11.4 W/m-K @Temperature 100 °C | 79.1 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 13.2 W/m-K @Temperature 200 °C | 91.6 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 15.0 W/m-K @Temperature 300 °C | 104 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 16.7 W/m-K @Temperature 400 °C | 116 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 18.4 W/m-K @Temperature 500 °C | 128 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 20.5 W/m-K @Temperature 600 °C | 142 BTU-in/hr-ft²-°F @Temperature 1110 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | <= 0.010 % | <= 0.010 % |
Chromium, Cr | 14 - 18 % | 14 - 18 % |
Cobalt, Co | <= 2.0 % | <= 2.0 % |
Iron, Fe | <= 3.0 % | <= 3.0 % |
Manganese, Mn | <= 1.0 % | <= 1.0 % |
Molybdenum, Mo | 14 - 17 % | 14 - 17 % |
Nickel, Ni | 58 % | 58 % |
Phosphorus, P | <= 0.025 % | <= 0.025 % |
Silicon, Si | <= 0.080 % | <= 0.080 % |
Sulfur, S | <= 0.010 % | <= 0.010 % |
Titanium, Ti | <= 0.70 % | <= 0.70 % |
|
Descriptive Properties |
---|
Average Oxidation Rate per 100-hour test period (mm) | 0.004 |
Thermal Diffusivity | 0.028 cm2/s |
| 0.031 cm2/s |
| 0.033 cm2/s |
| 0.037 cm2/s |
| 0.04 cm2/s |
| 0.043 cm2/s |
| 0.047 cm2/s |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.