MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chosun Refractories A80 Special High-Density Gunning Castable
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes:

Information provided by Chosun Refractories via Korea Institute of Ceramic Engineering and Technology (KICET).

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density  2.72 g/cc
@Temperature 1000 °C,
Time 10800 sec
0.0983 lb/in³
@Temperature 1830 °F,
Time 3.00 hour
 2.74 g/cc
@Temperature 110 °C,
Time 86400 sec
0.0990 lb/in³
@Temperature 230 °F,
Time 24.0 hour
 2.78 g/cc
@Temperature 1500 °C,
Time 10800 sec
0.100 lb/in³
@Temperature 2730 °F,
Time 3.00 hour
Porosity  15 %
@Temperature 110 °C,
Time 86400 sec
15 %
@Temperature 230 °F,
Time 24.0 hour
 16 %
@Temperature 1500 °C,
Time 10800 sec
16 %
@Temperature 2730 °F,
Time 3.00 hour
 19 %
@Temperature 1000 °C,
Time 10800 sec
19 %
@Temperature 1830 °F,
Time 3.00 hour
 
Mechanical PropertiesMetricEnglishComments
Modulus of Rupture  0.0073575 GPa
@Temperature 110 °C,
Time 86400 sec
1.0671 ksi
@Temperature 230 °F,
Time 24.0 hour
 0.010791 GPa
@Temperature 1000 °C,
Time 10800 sec
1.5651 ksi
@Temperature 1830 °F,
Time 3.00 hour
 0.01913 GPa
@Temperature 1500 °C,
Time 10800 sec
2.775 ksi
@Temperature 2730 °F,
Time 3.00 hour
 
Thermal PropertiesMetricEnglishComments
Shrinkage  -0.200 %
@Temperature 1500 °C,
Time 10800 sec
-0.200 %
@Temperature 2730 °F,
Time 3.00 hour
 -0.150 %
@Temperature 1000 °C,
Time 10800 sec
-0.150 %
@Temperature 1830 °F,
Time 3.00 hour
 -0.0500 %
@Temperature 110 °C,
Time 86400 sec
-0.0500 %
@Temperature 230 °F,
Time 24.0 hour
 
Component Elements PropertiesMetricEnglishComments
Al2O3 79 %79 %
SiO2 18 %18 %
 
Descriptive Properties
Main ApplicationsBlast furnace shaft
Material Required for Estimating (kg/m3)2,750

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Huntsman IROGRAN® A 85 E 4993 FCM Polyester-Based TPU-Injection Extrusion Grade
Chosun Refractories MRC-5 Blast Furnace Tap-Hole Refractory

CCHOS227 / 124171

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.