MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ICO Polymers ICOFLO™ 510-5028 400 Micron LLDPE Powder
Categories: Polymer; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE)

Material Notes: Description: ICOFLO 510-5028 is a premium polyethylene powder specifically designed to be used in the preparation of masterbatch (concentrate). By utilizing a free flowing powder as a carrier in masterbatch (instead of pellet), superior color development or additive dispersion can be achieved in the final concentrate.
Key Characteristics: very high melt flow and a linear low density polyethylene resin.

Information provided by ICO Polymers.

A Schulman acquired ICO, Inc. in 2010.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.926 g/cc0.0335 lb/in³ASTM D1505
Particle Size <= 400 µm<= 400 µmsieve < 5%
Melt Index of Compound 50 g/10 min
@Load 2.16 kg,
Temperature 190 °C
50 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 4848ASTM D2240
Tensile Modulus 0.0920 GPa13.3 ksi1 mm/min; ASTM D638
 
Thermal PropertiesMetricEnglishComments
Melting Point 121 °C250 °FDSC; ASTM D3418
Vicat Softening Point 92.0 °C198 °FASTM D1525

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ICO Polymers ICOFLO™ 510-5074 800 Micron LLDPE Powder
Dow 959S Linear Low Density Polyethylene (LDPE)
Dow GRSN-9820 NT 7 Linear Low Density Polyethylene Granular Solid
ICO Polymers ICOFLO™ 510-5069 400 Micron LLDPE Powder
ICO Polymers ICOFLO™ 510-5070 500 Micron LLDPE Powder

PICO009 / 47982

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.