Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.85 g/cc | 1.85 g/cc |
Mooney Viscosity | 27 @Temperature 121 °C | 27 @Temperature 250 °F |
| 45 @Temperature 100 °C | 45 @Temperature 212 °F |
| 75 @Temperature 100 °C | 75 @Temperature 212 °F |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore A | 65 | 65 |
| 60 @Time 3.00 sec | 60 @Time 0.000833 hour |
| 65 @Treatment Temp. 250 °C, Time 252000 sec | 65 @Treatment Temp. 482 °F, Time 70.0 hour |
| 65 @Treatment Temp. 275 °C, Time 252000 sec | 65 @Treatment Temp. 527 °F, Time 70.0 hour |
| 66 @Treatment Temp. 230 °C, Time 252000 sec | 66 @Treatment Temp. 446 °F, Time 70.0 hour |
Tensile Strength at Break | 14.2 MPa | 2060 psi |
| 10.2 MPa @Treatment Temp. 275 °C, Time 252000 sec | 1480 psi @Treatment Temp. 527 °F, Time 70.0 hour |
| 12.8 MPa @Treatment Temp. 250 °C, Time 252000 sec | 1860 psi @Treatment Temp. 482 °F, Time 70.0 hour |
| 13.5 MPa @Treatment Temp. 230 °C, Time 252000 sec | 1960 psi @Treatment Temp. 446 °F, Time 70.0 hour |
Elongation at Break | 340 % | 340 % |
| 354 % @Treatment Temp. 230 °C, Time 252000 sec | 354 % @Treatment Temp. 446 °F, Time 70.0 hour |
| 374 % @Treatment Temp. 250 °C, Time 252000 sec | 374 % @Treatment Temp. 482 °F, Time 70.0 hour |
| 418 % @Treatment Temp. 275 °C, Time 252000 sec | 418 % @Treatment Temp. 527 °F, Time 70.0 hour |
100% Modulus | 2.40 MPa @Strain 100 % | 348 psi @Strain 100 % |
Tear Strength | 36.0 kN/m | 205 pli |
Compression Set | 8.0 % @Temperature 100 °C, Time 252000 sec | 8.0 % @Temperature 212 °F, Time 70.0 hour |
| 9.0 % @Temperature 150 °C, Time 252000 sec | 9.0 % @Temperature 302 °F, Time 70.0 hour |
| 12 % @Temperature 50.0 °C, Time 252000 sec | 12 % @Temperature 122 °F, Time 70.0 hour |
| 12 % @Temperature 175 °C, Time 252000 sec | 12 % @Temperature 347 °F, Time 70.0 hour |
| 13 % @Temperature 25.0 °C, Time 252000 sec | 13 % @Temperature 77.0 °F, Time 70.0 hour |
| 21 % @Temperature 200 °C, Time 252000 sec | 21 % @Temperature 392 °F, Time 70.0 hour |
|
Thermal Properties | Metric | English | Comments |
---|
Minimum Service Temperature, Air | -18.0 °C | -0.400 °F |
| -15.0 °C | 5.00 °F |
| -10.0 °C | 14.0 °F |
| -9.00 °C | 15.8 °F |
Brittleness Temperature | -21.0 °C | -5.80 °F |
|
Processing Properties | Metric | English | Comments |
---|
Cure Time | 11.5 min @Temperature 160 °C | 0.192 hour @Temperature 320 °F |
| 15.0 min @Temperature 160 °C | 0.250 hour @Temperature 320 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Fluorine, F | 66 % | 66 % |
|
Descriptive Properties |
---|
Test Formula | 100 |
| 15 |
| 3 |
| 6 |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.